Vuam Hastelloy C276: Filler Hlau xaiv thiab txheej txheem tsim nyog

Jun 25, 2026

Tso lus

Hastelloy C276(UNS N10276, EN 2.4819) yog ib qho ntawm feem ntau corrosion-resistant nickel alloys muaj, dav siv nyob rau hauv chemical processing, roj & roj, tswj cov pa phem, thiab tshuaj industries. Txawm li cas los xij, nws qhov tshwj xeeb corrosion kuj tuaj yeem cuam tshuam los ntawm kev vuam tsis raug.

 

Tus yuam sij rau kev ua tiav C-276 fabrication yog xaiv cov hlau muab tub lim kom raug thiab tsim nyog rau cov txheej txheem vuam kom khaws cov hlau tsis sib xws - tshwj xeeb tshaj yog nws cov molybdenum siab thiab cov ntsiab lus carbon tsawg. Tsab ntawv xov xwm no muab cov lus qhia ua tiav rau kev xaiv cov khoom siv hlau, cov txheej txheem vuam, cov txheej txheem tsim nyog, thiab kev tswj xyuas zoo rau C276.

 

Welding Hastelloy C276

 

Siv ERNiCrMo-4 muab tub lim hlau rau sib piv C276 puag hlau. Tsim nyog cov txheej txheem vuam ntawm ASME Tshooj IX nrog tshuaj ntsuam xyuas ntawm cov hlau vuam los xyuas cov ntsiab lus Cr, Mo, thiab Fe. Tswj cov cua kub hauv qab 1.5 kJ / mm kom txo qis kev sib cais thiab khaws cia corrosion kuj.

 

Hastelloy C276 Taw qhia

 

Hastelloy C-276 yog npib tsib xee-molybdenum-chromium alloy nrog ntxiv ntawm tungsten. Nws cov yam ntxwv tseem ceeb yog cov ntsiab lus tsis tshua muaj carbon tsawg (tsawg dua lossis sib npaug li 0.01%), uas zoo li tshem tawm cov nag lossis daus carbide thaum vuam thiab kho cua sov. Qhov no ua rau C-276 resistant rau intergranular corrosion nyob rau hauv lub tshav kub-cuam tshuam cheeb tsam (HAZ) - ib tug teeb meem uas plagued qib ua ntej xws li Hastelloy C (UNS N10002).

 

Tshuaj muaj pes tsawg leeg

 

Rooj. Tshuaj muaj pes tsawg leeg ntawm Hastelloy C-276 (UNS N10276 / EN 2.4819)

                   

Lub ntsiab

Ni

Cr

Mo

Fe

W

Co

C

Si

Mn

Qhov hnyav%

Tshuav

14.5–16.5

15–17

4–7

3–4.5

Tsawg dua lossis sib npaug li 2.5

Tsawg dua lossis sib npaug li 0.01

Tsawg dua lossis sib npaug li 0.08

Tsawg dua los yog sib npaug rau 1.0

Lub luag haujlwm

Matrix

Oxidation kuj

Txo acid tsis kam

Kev txo nqi

Acid kuj

Cov seem

Minimized rau weldability

Minimized rau weldability

Deoxidizer

Source: ASTM B575-22 'Standard Specification for Nickel thiab Nickel-Cobalt Alloy Phaj, Sheet, thiab Sawb'; Haynes International 'HASTELLOY® C-276 Alloy' Daim Ntawv Qhia Cov Ntaub Ntawv (2023); Cov Khoom Tshwj Xeeb 'HASTELLOY® C-276' Phau Ntawv Qhia Khoom (2023).

 

Corrosion Resistance los ntawm Ib puag ncig

 

Rooj. Corrosion Resistance ntawm Hastelloy C-276 los ntawm ib puag ncig

           

Ib puag ncig

Corrosion hom

Nco ntsoov

Kub (degree)

Corrosion Rate (mm / xyoo)

Kev ntsuas

Hydrochloric acid (HCl)

General corrosion

1–37%

TSI – 70

< 0.13

Zoo heev

Sulfuric acid (H₂SO₄)

General corrosion

1–50%

TSI – 80

< 0.25

Zoo heev

Phosphoric acid (H₃PO₄)

General corrosion

1–85%

TSI – 100

< 0.10

Zoo heev

Hydrofluoric acid (HF)

General corrosion

1–48%

TSI – 50

< 0.50

Zoo

Nitric acid (HNO ₃)

Oxidizing corrosion

1–65%

TSI – 80

< 0.25

Zoo

Chlorine gas (ntub)

Pitting / crevice

Saturated

TSI – 100

< 0.10

Zoo heev

Dej hiav txwv

Pitting / crevice

3.5% Cl⁻

TSI – 100

< 0.01

Zoo heev

Cov kua qaub (H₂S)

SSC, SOHIC

pH₂S > 1 bar

TSI – 200

Tiv thaiv kab mob

Zoo heev

 

Source: Haynes International 'Corrosion Data for HASTELLOY® C-276' (2023); NACE Corrosion Data Survey, 6th Ed. (2020); Outokumpu 'Corrosion Handbook for Stainless Steels and Nickel Alloys' (2021).

 

C276 ua tau zoo hauv kev txo cov kua qaub (HCl, H₂SO₄) thiab chloride- muaj ib puag ncig uas cov hlau tsis huv. Nws cov ntsiab lus tsis tshua muaj carbon tshem tawm rhiab heev thaum vuam, ua rau nws yog qhov kev xaiv zoo tshaj plaws rau kev siv corrosion hnyav.

 

ERNiCrMo-4 Filler Hlau rau C276 Vuam

 

Rau vuam Hastelloy C-276, cov hlau muab tub lim yog ERNiCrMo-4 (AWS A5.14 classification). Cov hlau muab tub lim no muaj qhov tseem ceeb tib yam li C-276 lub hauv paus hlau, kom ntseeg tau tias cov hlau vuam muaj qhov sib txuam corrosion. Siv cov muab tub lim tsis raug - xws li ERNiCrMo-3 (Alloy 625) lossis ERNiCr-3 (Alloy 82) - yuav ua rau cov hlau txuas nrog qis molybdenum cov ntsiab lus thiab txo cov corrosion kuj hauv kev txo cov kua qaub.

 

ERNiCrMo-4 Filler Metal for C276 Welding

 

Rooj. Filler Hlau Xaiv rau Vuam Hastelloy C-276

               

AWS Class

UNS

Cr (%)

Mo (%)

Fe (%)

W (%)

C (%)

Kev pom zoo

ERNiCrMo-4

N10276

14.5–16.5

15–17

4–7

3–4.5

Tsawg dua los yog sib npaug li 0.02

✓ MATCHING - Kev xaiv thawj zaug

ERNiCrMo-10

N06022

20–22.5

12.5–14.5

2–6

2.5–3.5

Tsawg dua lossis sib npaug li 0.015

Alternative (siab dua Cr, qis Mo)

ERNiCrMo-14

N06686

19–23

15–17

Tsawg dua los yog sib npaug li 5

3–4.5

Tsawg dua lossis sib npaug li 0.01

Alternative (sib npaug Mo, siab dua Cr)

ERNiCrMo-3

N06625

20–23

8–10

Tsawg dua los yog sib npaug li 5

-

Tsawg dua lossis sib npaug li 0.10

✗ Tsis pom zoo (Mos Mo)

ERNiCr-3

N06082

18–22

-

Tsawg dua los yog sib npaug 3

-

Tsawg dua lossis sib npaug li 0.10

✗ TSIS pom zoo (tsis muaj Mo)

ERNiMo-7

N10665

Tsawg dua los yog sib npaug rau 1.0

26–30

Tsawg dua los yog sib npaug 2

-

Tsawg dua los yog sib npaug li 0.02

✗ TSIS pom zoo (tsis muaj Cr)

 

Source: AWS A5.14/A5.14M:2018 'Specification for Nickel and Nickel-Alloy Bare Welding Electrodes and Rods'; Haynes International 'HASTELLOY® C-276 Vuam Filler Metals' Technical Data (2023); Tshwj xeeb hlau 'Vuam Khoom Catalog' (2023).

 

Vim li cas ERNiCrMo-4 Yog Qhov Kev Xaiv Zoo

 

Kev tiv thaiv corrosion ntawm C-276 hauv kev txo cov kua qaub (HCl, H₂SO₄) nyob ntawm nws cov ntsiab lus molybdenum siab (15-17%). Yog tias siv cov khoom siv hlau nrog qis Mo, cov hlau welded yuav muaj kev tiv thaiv corrosion tsis zoo rau lub hauv paus hlau - tsim kom muaj 'tsis muaj zog txuas' hauv qhov sib koom ua ke. ERNiCrMo-3 (Alloy 625 muab tub lim) tsuas muaj 8-10% Mo, uas tsis txaus rau kev pabcuam acid txo qis.

 

Rooj. Kev cuam tshuam ntawm Filler Hlau Xaiv rau Weld Hlau Corrosion Resistance

           

Filler Hlau

Weld Hlau Mo (%)

HCl Corrosion Rate (mm / xyoo)

H₂SO₄ Corrosion Rate (mm/yr)

Seawater Pitting

Txiav txim

ERNiCrMo-4

15–17

< 0.13

< 0.25

Zoo heev

✓ TXOJ CAI

ERNiCrMo-10

12–14

< 0.25

< 0.50

Zoo heev

Txais tau rau oxidizing acids

ERNiCrMo-3

8–10

0.50–1.0

0.50–1.0

Zoo

✗ Tsis txaus rau txo cov kua qaub

ERNiCr-3

0

> 5.0

> 5.0

pluag

✗ TSIS MUAJ

Base Hlau C-276

15–17

< 0.13

< 0.25

Zoo heev

Kev siv

Source: Haynes International 'Corrosion Data for Weld Hlau ntawm HASTELLOY® Alloys' (2023); Cov Hlau Tshwj Xeeb 'Corrosion Resistance ntawm Nickel Alloy Welds' Technical Paper (2022); NACE Corrosion 2022 Lub Rooj Sib Tham Daim Ntawv 'Tshem Tawm Ntawm Cov Hlau Hlau Xaiv ntawm Nickel Alloy Weld Corrosion'.

 

Thaum Yuav Siv Cov Filler Hlau Ntau Lawm

 

Qee qhov xwm txheej, qhov siab dua - alloy muab tub lim hlau yuav raug teev kom them nyiaj rau kev sib cais los ntawm cov hlau hauv paus lossis muab cov npoo ntxiv. ERNiCrMo-14 (Alloy 686 muab tub lim) muaj Cr siab dua me ntsis thiab sib npaug Mo rau ERNiCrMo-4, ua rau nws tsim nyog rau cov ntawv thov uas yuav tsum tau muaj kev tiv thaiv corrosion siab tshaj.

 

Rooj. Overmatching Filler Hlau rau cov ntawv thov tseem ceeb

         

Filler Hlau

UNS

Cr (%)

Mo (%)

Daim ntawv thov

ERNiCrMo-14 (Alloy 686)

N06686

19–23

15–17

Kev sib tw rau C-276; dej hiav txwv, heev acids

ERNiCrMo-10 (Alloy C-22)

N06022

20–22.5

12.5–14.5

Overmatching rau oxidizing + txo cov sib tov

Tau qhov twg los: Haynes International 'HASTELLOY® ALLOY 686' Technical Data Sheet (2023); Cov Hlau Tshwj Xeeb 'INCONEL® ALLOY 686' Phau Ntawv Qhia Khoom (2023).

 

ERNiCrMo-4 yog qhov yuav tsum tau muab tub lim hlau rau vuam C-276 thaum yuav tsum tau ua kom muaj kev tiv thaiv corrosion. ERNiCrMo-14 lossis ERNiCrMo-10 tuaj yeem siv rau kev sib tsoo hauv cov ntawv thov tseem ceeb. Tsis txhob siv ERNiCrMo-3 (Alloy 625 muab tub lim) kom txo cov kua qaub.

 

GTAW and GMAW for C276

 

Hastelloy C276 tuaj yeem welded los ntawm tag nrho cov pa arc vuam txheej txheem, tab sis GTAW (TIG) thiab GMAW (MIG) yog cov feem ntau rau siab - kev ncaj ncees fabrication. GTAW muab kev tswj xyuas zoo tshaj plaws ntawm cov cua sov thiab cov khoom siv vuam tshuab, ua rau nws zoo tagnrho rau cov hauv paus hla thiab nyias ntu. GMAW muab cov khoom tsim tau ntau dua rau kev sau thiab lub hau hla hauv cov ntu tuab.

 

GTAW and GMAW for C276

 

Txheej Txheem Xaiv Phau Ntawv Qhia

 

Rooj. Vuam txheej txheem xaiv rau Hastelloy C-276

             

Txheej txheem

Txoj hauj lwm

Thickness Ntau

Thaum tshav kub kub input Control

Productivity

Daim ntawv thov

Kev pom zoo

GTAW (TIG)

Txhua txoj haujlwm

0.5-6 hli

Zoo heev

Tsawg

Hauv paus hla, nyias phab ntsa, orbital vuam

✓ Nyiam

GMAW (MIG)

Flat, kab rov tav

3-25 hli

Zoo

Nruab nrab

Sau thiab cap pass, khw fabrication

✓ Nyiam

PAW (Plasma)

Pav ca, orbital

1-10 hli

Zoo heev

Nruab nrab

Orbital raj vuam, precision welds

✓ Zoo

FCAW (Flux-Cored)

Flat, kab rov tav

5-30 hli

Ncaj ncees

Siab

Field fabrication, tsis yog - tseem ceeb

⚠ Siv ceev faj

SMAW (Stick)

Txhua txoj haujlwm

3-20 hli

pluag

Tsawg

Kev kho thaj chaw, tsis yog - tseem ceeb

⚠ Siv ceev faj

SAW (Submerged Arc)

Pav xwb

10-50 mm

pluag

Siab heev

Hnyav cladding, tsis yog - tseem ceeb

✗ Tsis pom zoo

Source: AWS D1.6/D1.6M-22 'Structural Welding Code-Stainless Steel'; Haynes International 'Welding Guidelines for HASTELLOY® C-276' (2023); ASME Boiler thiab Pressure Vessel Code Tshooj IX (2023).

 

GTAW Parameters C-276

 

Rooj. Pom zoo GTAW Parameters rau Hastelloy C-276

               

Thickness (hli)

Hom sib koom

Tam sim no (A)

Qhov hluav taws xob (V)

Kev ceev ceev (mm / min)

Hlau pub (mm / min)

Gas ntws (L / min)

Thaum tshav kub kub input (kJ / mm)

1.5

Square qab

50–70

9–11

120–150

300–400

8–12

0.3–0.5

3.0

V-groove 60 degree

80–110

10–12

100–130

400–500

10–15

0.5–0.8

6.0

V-groove 60 degree

120–150

11–13

80–100

500–600

12–18

0.8–1.2

10.0

V-groove 60 degree

150–180

12–14

70–90

600–700

15–20

1.0–1.5

12.0+

U-groov

160–200

12–14

60–80

600–800

15–20

1.2–1.5

Tau qhov twg los: Haynes International 'Welding Guidelines for HASTELLOY® C-276' (2023); Cov Hlau Tshwj Xeeb 'Vuam ntawm Nickel Alloys' Phau Ntawv Qhia (2023); ASME Section IX QW-409 'Vuam Variables-Electrical'.

 

Shielding Gas Xaiv

Rooj. Cov Lus Qhia Txog Kev Tiv Thaiv Gas rau C-276 Vuam

           

Txheej txheem

Thawj Gas

Flow tus nqi (L / min)

Thaub qab Gas

Tungsten electrode

Sau ntawv

GTAW

Argon (99.999%)

10–20

Argon lossis N₂ (yog tias xav tau)

2% Ceriated (EWCe-2)

Ntshiab Ar qhov tseem ceeb; tsis yog Nws rau hauv paus hla

GTAW (Hot Wire)

Argon + 5% H₂

12–18

Argon

2% Ceriated (EWCe-2)

H₂ nce cua sov; siv ceev faj

GMAW

Argon + 2–5% Nws

15–25

Argon

N/A

Nws txhim kho wetting; khaws tsawg dua lossis sib npaug li 5%

GMAW (Pulsed)

Argon + 2% Nws

12–20

Argon

N/A

Pulsed txo spatter; nyiam

PAW

Argon (99.999%)

3–5 (plasma) + 15–20 (cov ntaub thaiv npog)

Argon

2% Ceriated (EWCe-2)

Orbital vuam txheem

Source: AWS A5.32/A5.32M:2017 'Specification for Welding Shielding Gases'; Haynes International 'Welding Guidelines for HASTELLOY® C-276' (2023); Lincoln Electric 'Shielding Gas Xaiv rau Nickel Alloys' (2023).

 

GTAW with pure argon shielding is the preferred process for C-276 root passes and thin-wall applications. GMAW with Ar + 2–5% He is suitable for fill and cap passes. Avoid high helium mixtures (>10%) uas ua rau kom kub nkag thiab oxidation. Ib txwm siv siab - roj purity (99.999%) los tiv thaiv kev sib kis.

 

Thaum tshav kub kub input hauv qab 1.5 kJ / mm Yuav tsum tau kom txo qis kev sib cais

 

Txawm hais tias C-276 muaj cov pa roj carbon tsawg thiab tiv taus carbide nag lossis daus, cov cua kub ntau dhau tuaj yeem ua rau microsegregation ntawm molybdenum thiab chromium hauv cov hlau weld thiab HAZ. Qhov kev sib cais no tsim cov cheeb tsam hauv cheeb tsam nrog cov ntsiab lus ntawm cov hlau qis, txo cov kev tiv thaiv corrosion. Qhov kev pom zoo siab tshaj plaws cua sov yog 1.5 kJ / mm rau GTAW thiab 2.0 kJ / mm rau GMAW.

 

Thaum tshav kub kub input xam thiab txwv

 

Thaum tshav kub kub input yog xam raws li:

 

Formula:Kub input (kJ/mm)=Voltage (V) × Tam sim no (A) × 60 ÷ Travel Speed ​​(mm/min)

 

Rooj. Qhov ntsuas kub siab tshaj plaws rau C-276 Vuam

             

Txheej txheem

Max tshav kub input (kJ / mm)

Max Interpass Temp (degree)

Yog vim li cas

Cov nyhuv ntawm Kev Tshaj Tawm

Kev txo qis

Txuj

GTAW

1.5

175

Tsawg Mos cais

Txo corrosion kuj

Txo tam sim no, nce mus ncig ceev

Haynes, tshwj xeeb hlau

GMAW

2.0

175

Ib yam

Ib yam

Siv hom mem tes, stringer hlaws

Haynes, tshwj xeeb hlau

PAW

1.2

175

Precision tswj

Ib yam

Kho plasma tam sim no

Haynes

FCAW

2.5

175

Cov txheej txheem txwv

Tib + slag teeb meem

Tsis pom zoo rau qhov tseem ceeb

AWS D1.6

SMAW

3.0

175

Cov txheej txheem txwv

Tib + inclusions

Tsis pom zoo rau qhov tseem ceeb

AWS D1.6

Tau qhov twg los: Haynes International 'Welding Guidelines for HASTELLOY® C-276' (2023); Cov Hlau Tshwj Xeeb 'Vuam ntawm Nickel Alloys' Phau Ntawv Qhia (2023); AWS D1.6/D1.6M-22 'Structural Welding Code-Stainless Steel'.

 

Cov nyhuv ntawm tshav kub input rau Corrosion Resistance

 

Rooj. Cov nyhuv ntawm tshav kub nkag rau Weld Hlau Corrosion Resistance (ASTM G48 Method C)

         

Thaum tshav kub kub input (kJ / mm)

Weld Hlau Mo Segregation

CPT ( degree, ASTM G48)

CCT ( degree, ASTM G48)

Corrosion Rating

< 0.8

Tsawg kawg

> 85

> 60

Zoo heev

0.8–1.2

Tsawg

80–85

55–60

Zoo heev

1.2–1.5

Nruab nrab

70–80

45–55

Zoo

1.5–2.0

Qhov tseem ceeb

60–70

35–45

Txais tau

> 2.0

Siab

< 60

< 35

Degraded

 

Tau qhov twg los: ASTM G48-11 (2020) 'Txoj Kev Xeem Txheej Txheem rau Pitting thiab Crevice Corrosion Resistance ntawm Stainless Steels thiab Lwm Cov Alloys los ntawm Kev Siv Cov Tshuaj Ferric Chloride'; Haynes International 'Effect of Welding Thermal Cycles on C-276 Corrosion Resistance' Technical Paper (2022); NACE Corrosion 2021 Conference Paper.

 

Khaws cov cua kub hauv qab 1.5 kJ / mm rau GTAW thiab 2.0 kJ / mm rau GMAW. Siv stringer hlaws dai es tsis yog weaving. Tswj interpass kub hauv qab 175 degree. Txheeb xyuas qhov vuam hlau corrosion kuj los ntawm ASTM G48 kuaj thaum lub sij hawm tsim nyog.

 

ASME IX Cov Txheej Txheem Kev Tsim Nyog Yuav Tsum Muaj Tshuaj Ntsuam Xyuas thiab Kev Ntsuas Corrosion

 

Kev tsim nyog cov txheej txheem vuam rau Hastelloy C-276 rau ASME Tshooj IX yuav tsum muaj ntau tshaj li cov qauv kev ntsuas tshuab (tensile, khoov, cuam tshuam). Rau cov nickel alloys siv nyob rau hauv kev pab cuam corrosion, cov txheej txheem tsim nyog cov ntaub ntawv (PQR) yuav tsum muaj xws li tshuaj ntsuam xyuas ntawm cov hlau weld los xyuas kom meej tias Cr, Mo, thiab Fe cov ntsiab lus raws li cov specification. Kev kuaj corrosion ntxiv rau ASTM G48 tau pom zoo.

 

 

ASME IX Procedure Qualification Requires Chemical Analysis and Corrosion Testing

 

ASME IX Qhov tseem ceeb ntawm qhov hloov pauv rau C-276

 

Rooj. ASME IX Qhov Tseem Ceeb Ntawm Cov Vev Xaib rau C-276 Welding Procedure Qualification

         

Variable (QW-250)

Hloov Yuav Tsum Muaj Kev Tsim Nyog

Kev cuam tshuam rau C-276

Yuav tsum tau xeem

ASME IX Reference

Base Hlau (QW-403)

P-Tsis yog. 44 rau lwm tus P-Tsis yog.

Dilution hloov weld hlau chemistry

Tshuaj ntsuam xyuas

QW-403.1, QW-424

Filler Hlau (QW-404)

A-Tsis yog. los yog F-No. hloov; kev hloov pauv

Weld hlau chemistry

Tshuaj ntsuam xyuas

QW-404.5, QW-404.12

Vuam txheej txheem (QW-401)

Process change (GTAW to GMAW)

Thaum tshav kub kub input, dilution

Mechanical + chemical

QW-253

Thaum tshav kub kub input (QW-409)

Nce> 10%

Segregation, corrosion kuj

Corrosion Test (pom zoo)

QW-409.1

Position (QW-405)

Vertical-mus rau ntsug- nqes

Kub input hloov

Mechanical xeem

QW-405.1

Rov qab Gas (QW-408)

Hloov lossis tshem tawm

Hauv paus oxidation

Visual, tshuaj

QW-408.5

Ncej -Kev kho cua sov (QW-407)

Ntxiv lossis hloov

Cov tshuaj anneal yuav tsum tau

Mechanical, corrosion kuj

QW-407.1

Tau qhov twg los: ASME Boiler thiab Pressure Vessel Code Section IX (2023) QW-250 'Welding Variables'; QW-403 'Base Hlau'; QW-404 'Filler Hlau'; QW-409 'Electrical'; QW-424 'Base Hlau Groupings'; QW-442 'A-Number Classifications'.

 

Yuav tsum tau xeem rau C-276 PQR

Rooj. Yuav tsum tau xeem rau C-276 Welding Procedure Qualification

           

Kuaj

ASME IX Requirement

C-276 Cov Lus Qhia Tshwj Xeeb

Kev lees txais

Txoj Kev Xeem

Ntau zaus

Tensile Test

Yuav tsum tau (QW-150)

Ib yam

UTS Ntau dua lossis sib npaug rau 690 MPa

ASME IX QW-150

2 piv

Khoov Test

Yuav tsum tau (QW-160)

Ib yam

Tsis muaj kab nrib pleb> 3 mm

ASME IX QW-160

2 lub ntsej muag + 2 hauv paus

Impact Test

Yog xav tau los ntawm kev tsim

Thaum tsim kub

Rau ASME VIII

ASME IX QW-170

3 piv

Tshuaj ntsuam xyuas

Pom zoo (tsis tas yuav tsum tau)

✓ TSEEM CEEB rau C-276

Cr 14.5–16.5%, Mo 15–17%, Fe Tsawg dua lossis sib npaug li 7%

ASTM E1019, E1086

1 per PQR

Corrosion Test (ASTM G48)

Tsis xav tau los ntawm ASME IX

✓ YUAV TSUM PAUB TIAS

CPT Ntau dua lossis sib npaug li 75 degree, CCT Ntau dua lossis sib npaug li 50 degree

ASTM G48 Txoj Kev C

1 per PQR

Hardness Test

Yog xav tau los ntawm kev tsim

Rau kev pabcuam qaub (NACE MR0175)

Tsawg dua lossis sib npaug rau 22 HRC (weld + HAZ)

ASTM E10 / E18

5 nyeem ib cheeb tsam

Ferrite Number

Tsis siv tau

N/A (austenitic)

N/A

N/A

N/A

Source: ASME Boiler thiab Pressure Vessel Code Tshooj IX (2023) QW-150 'Tensile Test'; QW-160 'Bend Tests'; QW-170 'Ib Kev Ntsuas'; ASTM E1019-18 'Kev txiav txim siab ntawm Carbon, Sulfur, Nitrogen, thiab Oxygen hauv Hlau'; ASTM E1086-14 'Kev tshuaj xyuas ntawm Austenitic Stainless Steel los ntawm Spark Atomic Emission Spectrometry'; ASTM G48-11 (2020) 'Pitting thiab Crevice Corrosion Resistance'; NACE MR0175 / ISO 15156-3: 2015.

 

Kev Tshawb Fawb Txog Tshuaj

 

Kev tshuaj ntsuam xyuas cov hlau hlau yog qhov tseem ceeb tshaj plaws rau cov txheej txheem kev tsim nyog C-276. Kev tsom xam yuav tsum xyuas kom meej tias cov hlau weld ua tau raws li cov hauv qab no:

 

Rooj. Weld Metal Chemical Analysis Txais Cov Cai rau C-276

         

Lub ntsiab

Specification txwv

Hom Weld Hlau

Tseem ceeb rau

Txoj Kev Xeem

Chromium (Cr)

Ntau dua lossis sib npaug li 14.5%

15–16%

Oxidation kuj

OES, XRF, ICP

Molybdenum (hli)

Ntau dua lossis sib npaug li 15%

15.5–16.5%

Txo acid tsis kam

OES, XRF, ICP

Tungsten (W)

Ntau dua lossis sib npaug li 3.0%

3.2–3.8%

Acid kuj

OES, XRF, ICP

Hlau (Fe)

Tsawg dua lossis sib npaug li 7%

5–6%

Qhov taw qhia Dilution

OES, XRF, ICP

Cov pa roj carbon (C)

Tsawg dua lossis sib npaug li 0.02%

0.005–0.015%

Carbide nag lossis daus

Kev ntsuam xyuas combustion

Silicon (Si)

Tsawg dua lossis sib npaug li 0.20%

0.05–0.15%

Weldability

OES, XRF

Manganese (Mn)

Tsawg dua lossis sib npaug li 1.0%

0.3–0.6%

Deoxidation

OES, XRF

 

Tau qhov twg los: ASTM B575-22 'Specification for Nickel thiab Nickel-Cobalt Alloy Phaj, Sheet, thiab Sawb'; ASTM E1019-18 'Kev txiav txim siab ntawm Carbon, Sulfur, Nitrogen, thiab Oxygen'; ASTM E1086-14 'Kev tshuaj xyuas ntawm Austenitic Stainless Steel los ntawm Spark Atomic Emission Spectrometry'; ASTM E1621-21 'Elemental Analysis los ntawm Wavelength Dispersive X-Ray Fluorescence Spectrometry'.

 

Rau C-276 vuam txheej txheem tsim nyog, tshuaj ntsuam xyuas ntawm cov hlau vuam yog yuav tsum tau xyuas kom meej Mo, Cr, thiab Fe cov ntsiab lus. ASTM G48 corrosion test yog pom zoo rau cov kev pab cuam corrosion tseem ceeb. suav nrog cov kev xeem no hauv PQR thiab cov ntaub ntawv xeem cov ntaub ntawv.

 

Tshaj tawm - Weld Solution Annealing

 

Tsis zoo li austenitic stainless hlau, Hastelloy C-276 tsis xav tau kev kho cua sov tom qab vuam (PWHT) los kho corrosion vim nws cov ntsiab lus carbon tsawg tshem tawm qhov rhiab heev. Txawm li cas los xij, rau cov cheeb tsam uas muaj corrosive hnyav lossis thaum yuav tsum muaj kev tiv thaiv corrosion siab tshaj plaws, kev daws teeb meem ntawm 1120-1170℃tom qab txias txias yuav raug teev tseg.

 

Post-Weld Solution Annealing

 

PWHT Requirements rau C-276

 

Rooj. Tshaj tawm -Cov lus pom zoo kho cua sov rau Hastelloy C-276

         

Kev Pabcuam hnyav

Yuav tsum muaj PWHT?

Kev kho mob

Tau txais txiaj ntsig

Qhov tsis zoo

Nruab nrab corrosion (pH> 5)

Tsis muaj

Tsis muaj

Kev txuag nqi, tsis muaj kev cuam tshuam

Tsawg dua corrosion kuj

Corrosion hnyav (txo cov acids)

xaiv tau

Kev daws anneal 1120-1170 degree, dej quench

Maximum corrosion kuj, homogenized microstructure

Distortion txaus ntshai, ntxiv tus nqi

Cov kua qaub (H₂S)

Tsis muaj

Tsis muaj (NACE MR0175 tso cai raws li -welded)

Ua raws cai

Tsis muaj

Extreme corrosion (HF, kub HCl)

Pom zoo

Kev daws anneal 1150 degree, ceev txias

Tshem tawm microsegregation

Distortion txaus ntshai, rauv yuav tsum tau

Clad / weld overlay

Tsis muaj

Tsis muaj lossis kev ntxhov siab ntawm 650℃(yog tias xav tau)

Txo cov kev ntxhov siab seem

Tej zaum yuav cuam tshuam rau kev sib tshooj chemistry

Tau qhov twg los: Haynes International 'Kev Kho Mob Kub Kub ntawm HASTELLOY® C-276' Cov Lus Qhia (2023); ASME Boiler thiab Pressure Vessel Code Tshooj VIII Div. 1 (2023) UCS-56 'Requirements for Post-Weld Heat Treatment'; NACE MR0175 / ISO 15156-3: 2015.

 

Solution Annealing Parameters

Rooj. Tshuaj Annealing Parameters rau Hastelloy C-276

         

Parameter

Tus nqi

Lub hom phiaj

Tseem ceeb

Txuj

Kub

1120-1170 degree

Homogenize microstructure

Yog - yuav tsum tshaj 1120 degree

Haynes, ASTM B575

Tuav Sijhawm

10-30 feeb ib nti

Ua kom tiav

Yog - lub sij hawm tsis txaus=tsis tiav

Haynes

Huab cua

Cua los yog inert gas

Tiv thaiv oxidation

Yog - oxidizing cua ua rau nplai

Haynes

Txoj kev txias

Dej quench los yog cua txias sai

Tiv thaiv nag lossis daus

Yog - Kev txias qeeb ua rau muaj carbide tsim

Haynes, ASTM

Quench ncua

< 3 minutes

Tsis txhob muaj nag lossis daus

Yog - 870–650℃yog qhov tseem ceeb

Haynes

Tau qhov twg los: Haynes International 'Kev Kho Mob Kub Kub ntawm HASTELLOY® C-276' Cov Lus Qhia (2023); ASTM B575-22 'Specification rau Nickel thiab Nickel-Cobalt Alloy Phaj, Ntawv, thiab Sawb'; Cov Hlau Tshwj Xeeb 'Kev Kho Kub Kub ntawm Nickel Alloys' Phau Ntawv Qhia Kev Qhia (2023).

 

C-276 tsis xav tau PWHT rau feem ntau daim ntawv thov. Rau cov kev pab cuam corrosion heev, qhia cov tshuaj annealing ntawm 1150℃nrog dej quench. Tsis txhob qeeb-txias los ntawm 650-870℃qhov kub thiab txias, vim qhov no tuaj yeem ua rau nag lossis daus ntawm intermetallic theem.

 

PMI Verification thiab Corrosion Testing

 

Kev tswj xyuas zoo rau C-276 welds mus dhau tus qauv NDE (UT, RT, PT). Vim hais tias corrosion kuj nyob ntawm qhov tseeb chemistry, Positive Material Identification (PMI) ntawm cov hlau vuam yog qhov yuav tsum tau ua. Rau kev pabcuam corrosion tseem ceeb, ASTM G48 pitting thiab crevice corrosion testing yuav tsum suav nrog hauv cov txheej txheem tsim nyog.

 

Kev soj ntsuam thiab kev xeem yuav tsum tau

 

Rooj. Kev Tswj Xyuas Zoo rau Hastelloy C-276 Welds

             

Kuaj

Lub hom phiaj

Txoj kev

Kev lees txais

Ntau zaus

Txuj

Sau ntawv

PMI (Chemical)

Txheeb xyuas qhov vuam hlau chemistry

XRF lub OES

Mo Ntau dua lossis sib npaug rau 15%, Cr Ntau dua lossis sib npaug rau 14.5%, Fe Tsawg dua lossis sib npaug rau 7%

100% kev tsim khoom welds

ASTM E 1621 Cov Lus Qhia

Yuav tsum tau rau C-276

UT (Ultrasonic)

Pom tsis muaj fusion, porosity

Lub kaum sab xis

ASME VIII UW-51 lossis UW-52

Raws li specifications

ASME V Art . 4

Standard NDE

RT (Xov tooj cua)

Txheeb xyuas qhov tsis xws luag

X-ray lossis gamma

ASME VIII UW-51

Raws li specifications

ASME V Art . 2

Standard NDE

PT (Penetrant)

Nthuav cov kab nrib pleb

Pom pom lossis fluorescent zas xim

Tsis muaj linear indications> 1.5 mm

100% ntawm weld nto

ASME V Art . 6

Standard NDE

Hardness

Txheeb xyuas qhov ua raws NACE MR0175

Portable tester

Tsawg dua lossis sib npaug rau 22 HRC (weld + HAZ)

Rau NACE MR0175

ASTM E10 / E18

Rau kev pabcuam qaub

ASTM G48

Txheeb xyuas pitting kuj

Ferric chloride xeem

CPT Ntau dua lossis sib npaug li 75 degree, CCT Ntau dua lossis sib npaug li 50 degree

Rau PQR

ASTM G48 Txoj Kev C

Rau kev pabcuam tseem ceeb corrosion

Metallography

Tshawb xyuas microstructure

Hla -section, etch

Tsis muaj kab nrib pleb, porosity, los yog kev sib cais ntau dhau

Rau PQR

ASTM E3, E407, ASTM E3

Rau cov txheej txheem tsim nyog

 

Tau qhov twg los: ASTM E1621-21 'Elemental Analysis by Wavelength Dispersive X-Ray Fluorescence Spectrometry'; ASME Boiler thiab Pressure Vessel Code Tshooj V (2023) Tshooj 2, 4, 6; ASME Section VIII Div. 1 UW-51 'Radiographic Examination of Welds'; ASTM G48-11 (2020) 'Pitting thiab Crevice Corrosion Resistance'; NACE MR0175 / ISO 15156-3: 2015.

 

ASTM G48 Corrosion Test rau C-276

 

ASTM G48 yog tus qauv xeem txoj kev ntsuas pitting thiab crevice corrosion kuj. Rau C-276 weld hlau, Method C (Critical Pitting Temperature, CPT) los yog Method D (Critical Crevice Temperature, CCT) yuav tsum tau ua thaum lub sij hawm tsim nyog tus txheej txheem.

 

Rooj. ASTM G48 Corrosion Test Txais Cov Cai rau C-276 Weld Hlau

         

Txoj Kev Xeem

Test Solution

Qhov kub thiab txias

Txais tos rau C-276 Weld

Sau ntawv

Txoj kev C (CPT)

6% FeCl₃ + 1% HCl

25-95 ° C

CPT Ntau dua lossis sib npaug li 75 degree

Siab dua=zoo dua; puag hlau CPT> 85 degree

Txoj Kev D (CCT)

6% FeCl₃ + 1% HCl

25-85 ° C

CCT Ntau dua lossis sib npaug li 50 degree

Crevice hnyav dua; puag hlau CCT> 60 degree

Txoj Kev A (Qhov hnyav poob)

6% FeCl₃, 72h ntawm 22 degree

Kho qhov kub thiab txias

Qhov hnyav poob qis dua lossis sib npaug li 10 mg / cm²

Tsawg kev ntxub ntxaug rau C-276

Txoj Kev B (Crevice, yuag poob)

6% FeCl₃, 72h ntawm 22 degree

Kho qhov kub thiab txias

Qhov hnyav poob qis dua lossis sib npaug li 20 mg / cm²

Tsawg kev ntxub ntxaug rau C-276

 

Tau qhov twg los: ASTM G48-11 (2020) 'Txoj Kev Xeem Txheej Txheem rau Pitting thiab Crevice Corrosion Resistance ntawm Stainless Steels thiab Lwm Cov Alloys los ntawm Kev Siv Cov Tshuaj Ferric Chloride'; Haynes International 'Corrosion Testing of HASTELLOY® Alloys' Technical Guide (2023).

 

Kev txheeb xyuas PMI ntawm vuam hlau chemistry (Mo, Cr, Fe) yog qhov yuav tsum tau ua rau txhua qhov C-276 welds. Rau qhov kev pabcuam corrosion tseem ceeb, qhia ASTM G48 kuaj hauv cov txheej txheem tsim nyog. Txais CPT Ntau dua lossis sib npaug rau 75℃thiab CCT Ntau dua lossis sib npaug li 50℃raws li cov pov thawj ntawm kev tsim nyog weld hlau corrosion kuj.

 

C-276 Vuam Yuav tsum tau muab cov khoom sib txuam, tswj cov cua sov, thiab cov tshuaj muaj tseeb

 

Vuam Hastelloy C-276 tsis yooj yim, tab sis nws yuav tsum tau ua tib zoo saib rau peb yam tseem ceeb: (1) siv qhov sib txuam ERNiCrMo-4 muab tub lim hlau, (2) tswj cov cua kub hauv qab 1.5 kJ / mm kom txo qis kev sib cais, thiab (3) xyuas cov vuam hlau chemistry los ntawm PMI thiab corrosion kuj los ntawm ASTM G48 kuaj. Thaum cov kev cai no tau ua tiav, C-276 welds yuav muaj corrosion kuj sib npaug rau cov hlau puag.

 

Cov Lus Qhia Tseem Ceeb

 

  • Siv ERNiCrMo-4 (UNS N10276) muab tub lim rau kev sib piv C-276 puag hlau.
  • Tswj cov cua kub hauv qab 1.5 kJ / mm rau GTAW, 2.0 kJ / mm rau GMAW.
  • Siv cov roj ntshiab argon shielding (99.999%) rau GTAW; Ar + 2–5% Nws rau GMAW.
  • Khaws qhov kub ntawm qhov sib txawv hauv qab 175 degrees.
  • Ntxuav lub hauv paus hlau kom huv si nrog stainless hlau hlau txhuam; zam kev kis kab mob.
  • Tsim nyog cov txheej txheem vuam ib ASME IX nrog tshuaj ntsuam xyuas ntawm vuam hlau.
  • Txheeb xyuas Mo Ntau dua lossis sib npaug li 15%, Cr Ntau dua lossis sib npaug li 14.5%, Fe Tsawg dua lossis sib npaug li 7% hauv cov hlau vuam los ntawm PMI lossis kev soj ntsuam kuaj.
  • suav nrog ASTM G48 kev kuaj corrosion rau cov ntawv thov tseem ceeb heev.
  • Kev daws annealing tsis tas yuav tsum tau tab sis tej zaum yuav raug teev rau qhov kev pab cuam corrosion heev.
  • Sau tag nrho cov kev xeem thiab cov txiaj ntsig hauv daim ntawv tshaj tawm kev xeem (EN 10204 3.1 lossis 3.2)

 

Xa kev nug
Los rau peb
Thiab pib koj rfqs tam sim no.
Tiv Tauj Peb