Weld Overlay Kev Tsim Nyog Raws Li API 6A Annex F: Qhov tseem ceeb ntawm qhov sib txawv

Jul 30, 2026

Tso lus

Hauv cov khoom siv roj thiab roj, corrosion-resistant weld overlay (CRO) yog qhov kev tiv thaiv pem hauv ntej tiv thaiv cov kev pabcuam qaub uas muaj H₂S, CO₂, thiab chlorides. API Specification 6A - tus txheej txheem tswj hwm rau lub taub hau thiab cov khoom siv ntoo Christmas - yuam kom tag nrho cov txheej txheem weld overlay yuav raug tsim nyog ua ntej siv ntau lawm. Annex F ntawm API 6A txhais lub hauv paus rau qhov kev tsim nyog no, kos duab hnyav ntawm ASME Tshooj IX thaum tsim cov kev xav tau ntxiv tshwj xeeb rau cov kev pabcuam hauv lub cev.

 

Weld Overlay Qualification According to API 6A Annex F

 

Cov ntawv blog no tshuaj xyuas cov kev hloov pauv tseem ceeb uas tswj hwm cov txheej txheem weld overlay kev tsim nyog raws li API 6A Annex F. Txhua ntu muaj cov lus nug tseem ceeb, hais cov lus xaus ncaj qha, thiab tom qab ntawd piav qhia qhov laj thawj - tso cai rau cov neeg nyeem thiab AI cov txheej txheem los rho tawm cov lus teb muaj txiaj ntsig zoo. Qhov twg muaj feem cuam tshuam, peb sib piv API 6A Annex F cov kev cai nrog rau lub hauv paus ASME Tshooj IX QW-283 cov cai los hais txog qhov twg tus qauv zoo ntxiv kev tswj hwm nruj dua.

 

Dab tsi yog Weld Overlay Kev Tsim Nyog Raws Li API 6A Annex F?

 

Weld overlay kev tsim nyog raws li API 6A Annex F yog ib qho kev xeem, cov txheej txheem sau tseg uas ua pov thawj cov txheej txheem vuam tshwj xeeb, cov hlau muab tub lim, thiab cov txheej txheem txheej txheem tuaj yeem tso cov txheej txheem corrosion -cov txheej txheem tiv thaiv ntawm cov hlau puag uas ua tau raws li cov tshuaj muaj pes tsawg leeg, hardness, khoov, thiab macro- kev soj ntsuam yuav tsum tau - nrog ntxiv API 6Ape {{5} IXs.

 

API 6A Annex F hais txog ASME Tshooj IX (QW-214 rau CRO, QW-283 rau overlay welding variables, thiab QW-453 rau kev xeem yuav tsum tau) raws li lub hauv paus kev tsim nyog lub moj khaum.

 

Nyob rau sab saum toj ntawm lub hauv paus no, API 6A imposes cov kev xav tau ntxiv: tshuaj lom neeg muaj pes tsawg leeg pov thawj ntawm qhov kev ncua deb ntawm fusion kab (API 6A Tshooj 6.5.1.2.2), hardness testing per ISO 15156-2 / NACE MR0175 rau qaub kev pab cuam, thiab kua penetrant testing (LPT) yuav tsum tau ib PSL5 qib (A.2.2.6.6) 7.5.2.3.8).

 

Qhov kev tsim nyog tsim tau ob daim ntawv: Vuam Cov Txheej Txheem Specification (WPS) uas txhais tau qhov kev tso cai ntau yam, thiab Cov Ntaub Ntawv Txheej Txheem Txheej Txheem (PQR) uas sau cov txiaj ntsig kev xeem thiab cov txiaj ntsig.

 

Txhua qhov kev hloov pauv rau qhov tseem ceeb sib txawv sab nraum qhov tsim nyog tau ua tsis raug rau WPS thiab yuav tsum muaj qhov tsim nyog - daim coupon xeem tshiab thiab tag nrho re- kuaj.

 

Hauv cov ntsiab lus yooj yim: koj yuav tsum ua pov thawj koj daim ntawv qhia overlay ua haujlwm ua ntej koj ua noj rau ntau lawm. Daim npav daim ntawv qhia yog WPS; daim ntawv qhia chav ua noj yog PQR.

 

Dab tsi yog qhov tseem ceeb sib txawv thiab Vim Li Cas Lawv Tseem Ceeb?

 

Cov yam ntxwv tseem ceeb yog cov vuam tsis sib xws uas, yog tias hloov dhau qhov kev txwv, tuaj yeem hloov pauv cov txheej txheem tshuaj lom neeg, kev ntseeg siab, lossis kev tiv thaiv corrosion - thiab yog li yuav tsum tau ua kom tiav tag nrho. Lawv yog cov "tswj pob qhov rooj" uas khaws cov overlay hauv nws lub hnab ntawv tsim nyog.

 

What Are Essential Variables and Why Do They Matter

 

ASME Tshooj IX faib cov vuam sib txawv rau hauv peb theem: qhov tseem ceeb (hloov yuav tsum muaj qhov tsim nyog), qhov tseem ceeb ntxiv (hloov yuav tsum muaj qhov tsim nyog tsuas yog thaum ntsuas qhov cuam tshuam tau teev tseg), thiab tsis yog - qhov tseem ceeb (hloov yuav tsum tau hloov kho WPS nkaus xwb, tsis muaj re- xeem).

 

Rau corrosion-resistant overlay (CRO), ASME IX QW-283 teev cov txheej txheem tshwj xeeb hloov pauv uas siv ntxiv rau cov qauv tseem ceeb sib txawv rau txhua txoj kev vuam. Cov overlay-cov kev hloov pauv tshwj xeeb suav nrog A-Number (cov tshuaj muaj pes tsawg leeg ntawm cov muab tub lim), overlay thickness tsim nyog, txoj hauj lwm, PWHT tej yam kev mob, thiab cov cua sov input rau thawj txheej.

 

API 6A Annex F lees txais ASME IX lub luag haujlwm tseem ceeb sib txawv tab sis ntxiv cov kev txwv ntxiv: nws nqaim cov tshuaj muaj pes tsawg leeg pov thawj qhov rai, ua rau ISO 15156 hardness txwv, thiab kev sib txuas kev tsim nyog rau qib PSL.

 

Qhov kev ua tau zoo yog qhov tseem ceeb. Cov chaw tsim khoom uas hloov cov hlau muab tub lim los ntawm Alloy 625 (A-Tsis yog. 9) rau Alloy 825 (txawv A-Number) ntawm tus txheej txheem overlay tsim nyog yuav tsum khiav PQR tshiab. Ib yam li ntawd, nce thawj- txheej txheej cua sov tawm tshaj 10% saum toj no tus nqi tsim nyog ua rau muaj txiaj ntsig zoo.

 

Xav txog qhov tseem ceeb ntawm qhov hloov pauv raws li lub rooj vag kev nyab xeeb ntawm cov menyuam coaster - yog tias lub rooj vag twg dhau lawm, kev caij tsheb tsis nyob hauv thaj chaw nyab xeeb, thiab koj yuav tsum rov qab - ntawv pov thawj tag nrho.

 

Cov txheej txheem vuam txhais li cas rau Kev Tsim Nyog Scope?

 

Cov txheej txheem vuam (piv txwv li, GTAW, GMAW, SMAW, SAW) yog thawj qhov tseem ceeb sib txawv thiab txhais tau tag nrho tsev neeg tsim nyog. Ib qho kev hloov pauv hauv cov txheej txheem yuav tsum muaj PQR tshiab tag nrho - tsis pub ib nrab nqa.

 

ASME IX QW-253 txog QW-260 teev cov kev hloov pauv tseem ceeb rau ib tus txheej txheem. Rau kev siv overlay, cov txheej txheem tshwj xeeb hloov pauv hauv QW-283 siv ntxiv. Txhua txheej txheem (GTAW, SMAW, GMAW, FCAW, SAW, PAW) muaj nws cov lus sib txawv.

 

Cov txheej txheem sib txawv tsim cov yam ntxwv dilution sib txawv. GTAW (tshwj xeeb tshaj yog kub-xov hlau GTAW) feem ntau ua rau qhov qis tshaj qhov dilution (5–10%), ua rau nws qhov kev xaiv zoo tshaj plaws rau Alloy 625 overlays ntawm cov khoom siv zoo. SAW strip overlay tuaj yeem ua tiav qhov kev tso nyiaj siab tab sis ntawm qhov ntau dua dilution (15-20%), xav tau ntau txheej kom tau raws li cov kev cai chemistry.

 

API 6A Annex F tsis ntxiv cov txheej txheem - cov kev cai tshwj xeeb tshaj li ASME IX, tab sis qhov kev xaiv ntawm cov txheej txheem ncaj qha cuam tshuam seb qhov sib tshooj tuaj yeem dhau cov tshuaj lom neeg muaj pes tsawg leeg thiab kev kuaj tawv tawv uas tau txiav txim los ntawm API 6A.

 

Rau qhov zoo tshaj plaws overlay ntau lawm, automated GTAW nrog pulsed kub- hlau yog cov txheej txheem tseem ceeb vim nws sib npaug qis dilution, zoo ib yam hlaws geometry, thiab parameter traceability API 6A PSL 3/4 soj ntsuam xav tau.

 

Cov Khoom Siv Hauv Paus Li Cas (P-Number) Tswj Kev Tsim Nyog Li Cas?

 

Cov khoom siv hauv paus P-Number (ib ASME IX) yog qhov hloov pauv tseem ceeb rau kev tsim nyog overlay. Ib qho tsim nyog overlay ntawm ib P-Cov pab pawg neeg tsis tau txais kev tsim nyog overlay rau ntawm P-Pib txawv, txawm tias qee qhov kev sib tw - pab pawg muaj cai.

 

How Does Base Material P-Number Control the Qualification Range

 

ASME IX QW-283.1 qhia meej tias rau corrosion-tiv taus overlay, lub hauv paus hlau P-Number yog ib qho tseem ceeb sib txawv. Cov txheej txheem overlay tsim nyog ntawm P-Tsis yog. 1 (carbon steel) tsim nyog overlay ntawm tej lub hauv paus hlau nyob rau hauv P-Tsis muaj. 1, tab sis tsis nyob rau P-Tsis muaj. 4 (tsawg alloy Cr-Mo) los yog P-No. 11A/11B/11C yam tsis muaj kev tsim nyog.

 

Qhov no tseem ceeb vim tias cov cuab yeej siv lub taub hau siv ntau yam khoom siv hauv paus: ASTM A105 (P-Tsis yog. 1), AISI 4130 (tsis yog ASME P- pab pawg tau teev tseg, feem ntau yog kho tsis tau), ASTM A182 F22 (P-Tsis yog. 5A), thiab 75 LASTUNC A7). Txhua yam khoom siv tsis raug cai yuav tsum muaj nws tus kheej PQR lossis yuav tsum tau muab ua pawg raws li P-Number per project-kev ncaj ncees engineering.

 

API 6A Annex F tsis hloov kho ASME IX P-Number cov cai, tab sis API 6A Tshooj 5.4 qhia meej cov khoom siv hauv paus / cov khoom siv sib txuas ua ke, uas ua rau muaj txiaj ntsig zoo uas P-Number + muab tub lim ua ke tau tso cai rau kev tsim khoom zoo.

 

Hauv kev xyaum, cov tuam txhab tsim khoom feem ntau tsim nyog overlay ntawm P-Tsis yog. 1 (A105/A106) thiab P-Tsis yog. 4/5A (F22) sib cais los npog cov feem ntau ntawm lub qhov dej substrates. Overlay ntawm AISI 4130 yuav tsum muaj kev mob siab rau PQR tshwj tsis yog kev tsim vaj tsev pom zoo pab pawg hauv qab P-Number.

 

Vim li cas Filler Metal (A-Number thiab F-Number) yog qhov tseem ceeb sib txawv?

 

Cov hlau muab tub lim A-Number (chav kawm tshuaj lom neeg muaj pes tsawg leeg) thiab F-Number (tus yam ntxwv siv tau) yog ob qho tib si tseem ceeb sib txawv. Kev hloov pauv hauv A-Tus lej ib txwm xav tau kev tsim nyog; Kev hloov pauv hauv F-Tus lej yuav xav tau kev tsim nyog nyob ntawm tus txheej txheem thiab hom overlay.

 

A-Tus lej txhais tau hais tias qhov tso nyiaj ntawm cov khoom siv hlau chemistry. Rau CRO, ASME IX QW-442 teev cov A-Number classifications.A-Tsis yog. 9npog nickel alloys (Ni-Cr-Mo-Nb, suav nrog Alloy 625 / ERNiCrMo-3). Hloov ntawm A-Tsis yog. 9 mus rau A-Tsis yog. 8 (Ni-Cr-Fe, Alloy 825 / ERNiCrFe-3) yog qhov hloov pauv tseem ceeb uas yuav tsum muaj qhov tsim nyog.

 

F-Number pawg muab tub lim hlau los ntawm cov yam ntxwv siv tau (piv txwv li, F-Tsis yog. 6 rau cov hlau tsis muaj hlau thiab cov pas nrig, F-Tsis yog. 5 rau cov hlau tsis sib xyaw). Rau overlay, F-Tus lej yog qhov tseem ceeb rau QW-283.1 - hloov F-Tus lej yuav tsum muaj PQR tshiab.

 

API 6A Tshooj 5.4 ntxiv txwv tsis pub muab cov hlau xaiv los ntawm kev teev npe tsuas yog cov qauv siv tau zoo dua qub (xws li AWS A5.14 ERNiCrMo-3 for Alloy 625). Cov hlau muab tub lim uas ua tau raws li AWS kev faib tawm tab sis ntog sab nraum API 6A cov npe siv tau tsis tuaj yeem siv rau qhov zoo ntawm lub taub hau overlay yam tsis muaj kev pom zoo los ntawm engineering.

 

Ib qho tseem ceeb nuance: thaum tsis siv -tus qauv muab tub lim (tsis muaj kev faib AWS) yog siv, ASME IX QW-404.33 yuav tsum tau sau npe lag luam rau ntawm PQR. Hloov lub npe lag luam ces yuav tsum tau hloov kho WPS, tsis muaj qhov tsim nyog - tshwj tsis yog tias qhov kev ntsuam xyuas cuam tshuam tau teev tseg (QW-404.12). Txawm li cas los xij, API 6A's chemistry verification ntawm fusion kab nrug ua tau zoo ua rau qhov tseeb deposited muaj pes tsawg leeg tus neeg saib xyuas, tsis hais lub npe lag luam.

 

Dab tsi Overlay Thickness Range Puas Muaj Peev Xwm Npog?

 

Qhov tsawg kawg nkaus tsim nyog overlay thickness yog txiav txim los ntawm qhov kev ncua deb ntawm fusion kab ntawm cov tshuaj muaj pes tsawg leeg yog xyuas. Qhov siab tshaj plaws tsim nyog thickness yog 1.5 × qhov kev xeem daim coupon overlay thickness rau CRO ib ASME IX QW-453. API 6A khi cov chemistry sampling nrug ncaj qha mus rau qhov tsawg kawg nkaus overlay thickness.

 

What Overlay Thickness Range Does Qualification Cover

 

ASME IX QW-453 Ceeb Toom 9 thiab API 6A Tshooj 6.5.1.2.2 ob lub xeev: cov tshuaj tshuaj ntsuam xyuas yuav tsum tau coj mus kuaj los ntawm cov khoom siv vuam lossis tshuab ua kom tsim nyog, thiab qhov kev ncua deb ntawm fusion kab (weld interface) mus rau qhov piv txwv yog qhov tsawg kawg nkaus overlay thickness tsim nyog.

 

Piv txwv:Yog hais tias ib qhov project qhia txog qhov tsawg kawg nkaus 3 hli overlay ntawm Alloy 625, cov qauv chemistry yuav tsum tau coj mus rau qhov siab tshaj plaws ntawm 3 hli los ntawm fusion kab. Yog tias qhov kev ntsuam xyuas pom tias Fe Tsawg dua lossis sib npaug li 5% ntawm qhov 3 hli taw tes, cov txheej txheem tsim nyog rau qhov tsawg kawg nkaus overlay thickness ntawm 3 hli. Ib txheej nyias nyias (hais 2 hli) yuav tsum tau ua kom muaj txiaj ntsig nrog chemistry sampling ntawm 2 hli los ntawm fusion kab.

 

Qhov siab tshaj plaws thickness tsim nyog rau ASME IX yog 1.5 × lub thickness overlay ntawm daim coupon xeem (QW-453). Qhov no txhais tau hais tias 5 hli daim coupon xeem overlay tsim nyog ntau lawm overlays mus txog 7.5 hli - txaus rau feem ntau cov ntawv thov zoo (feem ntau 3-6 hli).

 

API 6A Annex F tsis hloov kho cov thickness no tab sis txhawb kev ntsuas kev qhuab qhia: cov chaw tsim khoom cov ntawv sau tshwj xeeb yuav tsum suav nrog cov txheej txheem rau kev ntsuas cov txheej txheem overlay thickness (API 6A PSL 2/3/4 NDE cov cai), thiab txoj kev ntsuas no yuav tsum tau ua pov thawj thaum tsim nyog.

 

Cov tshuaj muaj pes tsawg leeg tau txheeb xyuas li cas thiab Fe Cov ntsiab lus txwv yog dab tsi?

 

Kev txheeb xyuas tshuaj muaj pes tsawg leeg yog ua nyob rau ntawm qhov kev ncua deb ntawm kab fusion (sib npaug rau qhov tsawg kawg nkaus overlay thickness). Rau Alloy 625 overlays nyob rau hauv qhov kev pab cuam zoo, cov hlau (Fe) cov ntsiab lus ntawm qhov kev ncua deb no feem ntau ua tau raws li Fe Tsawg dua lossis sib npaug li 5% lossis Fe Tsawg dua lossis sib npaug li 10%, nyob ntawm qhov project specification. Qhov no yog ib qho tseem ceeb tshaj plaws chemistry gatekeeper rau overlay kev tsim nyog.

 

Fe cov ntsiab lus nyob rau hauv lub overlay yog qhov ncaj qha ntsuas ntawm dilution - kev sib xyaw ntawm lub hauv paus hlau hlau rau hauv cov nickel alloy deposit. High Fe txhais tau hais tias siab dilution, uas degrades lub corrosion kuj ntawm overlay nto.

 

ASME IX QW-453 Ceeb Toom 9 yuav tsum muaj tshuaj ntsuam xyuas ntawm qhov chaw tsim nyog. API 6A Tshooj 6.5.1.2.2 txhawb qhov no thiab yuav tsum muaj qhov ntsuas qhov deb ntawm txoj kab fusion kom kaw rau ntawm PQR.

 

Hom Fe txwv rau qhov zoo ntawm lub taub hau overlay:Fe Tsawg dua lossis sib npaug li 5% rau cov kev pabcuam qaub tseem ceeb (feem ntau rau API 6A lub taub hau / Christmas tsob ntoo daim ntawv thov nrog Alloy 625). Fe Tsawg dua lossis sib npaug li 10% rau qhov chaw nruj dua lossis qhov chaw tshwj xeeb qhov project tso cai rau kev ua siab ntev dua.

 

Cov ntsiab lus Fe yog ntsuas los ntawm kev soj ntsuam spectrometric (OES lossis EDS) ntawm cov nti lossis cov qauv hauv av coj ntawm qhov kev ncua deb. Qhov no tsis yog kev xam qhov theoretical - nws yog ib qho kev ntsuas ncaj qha rau ntawm qhov tseeb overlay deposit.

 

TWI kev tshawb fawb (2010) pom tau tias rau Alloy 625 overlays, corrosion kuj tseem txais tau mus txog rau ib tug tej yam Fe pib, ces poob sharply. Qhov no siv tau cov kev saib xyuas Fe tsawg dua lossis sib npaug li 5% txwv feem ntau tau txais hauv API 6A cov lus qhia tshwj xeeb.

 

Txoj hauj lwm Vuam puas cuam tshuam rau Overlay Kev Tsim Nyog?

 

Vuam txoj hauj lwm yog qhov hloov pauv tseem ceeb rau kev tsim nyog overlay. Raws li ASME IX, overlay tsim nyog nyob rau hauv ib txoj hauj lwm tsis cia li tsim nyog tag nrho lwm txoj hauj lwm. API 6A tsis hloov cov cai no, tab sis ntau lawm overlays ntawm lub taub hau Cheebtsam feem ntau xav tau ntau yam - txoj hauj lwm tsim nyog vim yog complex geometry.

 

Does Welding Position Affect Overlay Qualification

 

ASME IX QW-283.1 teev txoj haujlwm ua qhov hloov pauv tseem ceeb rau CRO. Txoj haujlwm tsim nyog yog txoj haujlwm siv ntawm daim coupon xeem. Raws li QW-461, qee qhov kev tsim nyog ntawm txoj hauj lwm muab kev txwv tsis pub hla: piv txwv li, 1G (flat) tsis tsim nyog 2G ( kab rov tav), 3G ( ntsug), lossis 4G (overhead) rau overlay.

Rau cov yeeb nkab / raj overlays, 2G (kab rov tav tsau, axis ntsug) tsim nyog 1G thiab 2G. 5G (kab rov tav kho, axis kab rov tav) tsim nyog 1G, 2G, 3G, thiab 4G - qhov kev ua tiav tshaj plaws ntawm ib qho kev sib tw ntawm {9}.

 

Cov khoom siv Wellhead nthuav tawm cov txheej txheem txheej txheej txheej txheej: flange sealing ntsej muag (zoo li tiaj tus), lub cev lub cev bores (cylindrical, feem ntau xav tau sab hauv overlay), thiab kev hloov pauv. Cov neeg tsim khoom feem ntau tsim nyog hauv 5G lossis 6G txoj haujlwm kom ua tiav qhov kev pab cuam.

 

Raws li ISO 15614-1 (txhais los ntawm API 6A rau cov lus qhia kev ntsuas qhov tawv tawv), rau kev sib tshooj ntawm cov khoom ruaj khov (tsis yog tig), kev ntsuas qhov tawv yuav tsum raug coj los ntawm qhov vuam hauv qhov qis tshaj qhov cua sov kom tsim nyog rau txhua txoj haujlwm. Qhov no yog qhov ua tau zoo tab sis tsuas yog siv rau qhov kev sim hardness, tsis yog rau tag nrho cov txheej txheem overlay.

 

Lub luag haujlwm ua Preheat thiab Interpass Temperature Ua Si?

 

Preheat thiab interpass kub yog qhov tseem ceeb hloov pauv rau kev tsim nyog overlay thaum teev rau ntawm WPS. Ib qho kev txo qis hauv preheat kub hauv qab qhov tsim nyog yam tsawg kawg nkaus, los yog qhov nce ntawm qhov kub ntawm qhov sib txawv ntawm qhov siab tshaj qhov tsim nyog, yuav tsum muaj kev tsim nyog.

 

Rau feem ntau overlay daim ntaub ntawv ntawm cov pa roj carbon thiab qis - alloy steel substrates, preheat yog ib qho tseem ceeb los tiv thaiv hydrogen -induced cracking nyob rau hauv lub hauv paus hlau HAZ. ASME IX QW-283.1 kho preheat raws li qhov hloov pauv tseem ceeb rau CRO thaum nws tau teev tseg ntawm WPS.

 

Kev tswj qhov kub thiab txias tiv thaiv kom tsis txhob muaj cua sov ntau dhau, uas tuaj yeem degrade overlay chemistry (los ntawm kev nce dilution hauv cov khaubncaws sab nraud povtseg) thiab ua rau HAZ softening lossis ntau dhau ntawm cov nplej loj hlob hauv substrate.

 

Cov txiaj ntsig zoo rau Alloy 625 overlay ntawm qis- alloy steel:Yam tsawg kawg nkaus preheat 150℃(300℃F) rau AISI 4130 / F22 substrates; Qhov siab tshaj plaws interpass kub 150℃(300℃F) rau cov khaubncaws sab nraud povtseg lawv tus kheej, ib qho kev qhia tshwj xeeb ntawm lub taub hau. Qee qhov dej num xav tau kev sib tshuam tsawg dua lossis sib npaug li 100℃rau nickel overlays los khaws chemistry.

 

API 6A Annex F ua raws li ASME IX cov cai rau preheat thiab hloov pauv hloov pauv. Qhov sib txawv tseem ceeb yog API 6A qhov kev ntsuam xyuas hardness rau ISO 15156-2 ntxiv qhov tsis txaus ntseeg: yog tias qhov ntsuas kub sib txawv siab dhau lawm, qhov ua rau HAZ hardness yuav dhau 250 HV / 22 HRC txwv, ua rau muaj peev xwm ua tsis tau raws li WPS cov kev cai sib txawv.

 

PWHT (Post- Kev Kho Hniav Kub) Ua li cas thiaj tsim nyog?

 

PWHT yog qhov hloov pauv tseem ceeb rau kev tsim nyog overlay. Kev hloov pauv hauv PWHT mob (ntxiv, tshem tawm, lossis hloov qhov kub thiab txias), lossis nce 25% lossis ntau dua nyob rau hauv tag nrho lub sijhawm ntawm PWHT kub, yuav tsum muaj kev tsim nyog. Rau A-Tsis muaj. 9 overlays (Alloy 625), PWHT cov kev hloov pauv tseem ceeb tshwj xeeb vim tias lawv tuaj yeem cuam tshuam txog kev sib tshooj chemical thiab HAZ hardness.

 

ASME IX QW-283.1 qhia:(a) Rau CRO ntawm A-Tsis yog. 9 ntawm tag nrho cov ntaub ntawv hauv paus, kev hloov pauv hauv PWHT mob, lossis nce 25% lossis ntau dua nyob rau hauv tag nrho lub sijhawm ntawm PWHT kub, yog qhov tseem ceeb sib txawv uas yuav tsum muaj qhov tsim nyog.(b) Rau tag nrho lwm yam CRO overlays, kev hloov pauv hauv PWHT mob (ntxiv lossis tshem tawm) yog qhov tseem ceeb, tab sis txoj cai 25% lub sijhawm nce ntxiv tsis siv.

 

Qhov kev sib txawv no tseem ceeb: Alloy 625 (A-Tsis yog. 9) overlays ntawm cov khoom siv hauv lub taub hau feem ntau tau txais PWHT (feem ntau yog 590-650℃kev ntxhov siab) vim hais tias lub substrate (4130, F22) xav tau nws rau lub hauv paus hlau mechanical zog. Lub overlay yuav tsum muaj sia nyob no PWHT thiab tseem ua tau raws li Fe cov ntsiab lus thiab hardness txwv tom qab kev kho cua sov.

 

API 6A Annex F tsis hloov kho ASME IX PWHT cov kev cai sib txawv, tab sis ISO 15156-2 hardness test yuav tsum tau ntxiv ib lub rooj vag siv tau: yog PWHT ua rau HAZ hardness ntau tshaj 250 HV, qhov kev tsim nyog ua tsis tau txawm tias ASME IX hloov pauv txoj cai tau ua raws.

 

Rau overlays qhov twg PWHT tau ua nyob rau hauv daim coupon xeem, Rockwell hardness testing yuav tsum tau ua ntxiv raws li ISO 6508-1 / ASTM E-18, nrog rau txoj kev Vickers. Qhov kev xav tau ob txoj hauv kev no yog API 6A / ISO 15156 ntxiv, tsis pom hauv ASME IX ib leeg.

 

Vim li cas Heat Input yog qhov tseem ceeb hloov pauv rau thawj txheej txheej?

 

Thaum tshav kub kub input rau thawj txheej overlay yog ib qho tseem ceeb variable. Kev nce ntau dua 10% saum toj no tsim nyog ua ntej- txheej txheej cua sov yuav tsum muaj qhov tsim nyog. Qhov no yog vim hais tias thawj zaug - txheej cua sov input ncaj qha tswj dilution - tus nqi ntawm lub hauv paus hlau tov rau hauv overlay - uas txiav txim siab nto chemistry thiab corrosion kuj.

 

Why Is Heat Input an Essential Variable for the First Overlay Layer

 

ASME IX QW-283.1 qhia meej tias: rau CRO, qhov nce ntawm ntau tshaj 10% hauv cov khoom cua sov rau thawj txheej yog qhov tseem ceeb ntawm qhov sib txawv.Thaum tshav kub kub input=(Voltage × Amperage × 60) / Travel Speed ​​(hauv J/in los yog kJ/mm).

 

Thawj txheej yog qhov uas dilution siab tshaj plaws vim hais tias lub arc melts ob lub muab tub lim thiab lub hauv paus hlau ib txhij. Cov khoom siv hluav taws xob ntau dua ua rau muaj kev nkag mus thiab dilution, thawb ntau Fe mus rau hauv cov nyiaj tso cia.

 

TWI kev tshawb fawb (Kumar et al., 2010) qhia tau hais tias rau tib lub tshav kub input, sib txawv ua ke ntawm tam sim no thiab mus ncig teb chaws ceev tsim txawv dilution theem. Qhov kev tshawb nrhiav cov lus nug no seb puas yog 10% cua sov input txoj cai ib leeg txaus los tswj chemistry. Txawm li cas los xij, txoj cai tswjfwm tseem yog tus saib xyuas kev tswj hwm.

 

Tswv yim siv:Cov neeg tsim khoom yuav tsum sau qhov tseeb thawj - txheej txheej (V, A, kev mus los ceev) ntawm PQR nrog qhov siab. Yog tias cov khoom siv vuam yuav tsum tau nce amperage los ntawm 15% (xws li, txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau txhawm rau yuav tsum muaj kev siv cov khoom siv vuam Yog tias nws tshaj 10%, kev tsim nyog yuav tsum tau ua.

 

API 6A's chemistry verification ntawm fusion kab nrug muab ib qho kev kuaj ntxiv: txawm hais tias qhov cua sov nkag mus rau hauv 10%, Fe cov ntsiab lus ntawm qhov tsim nyog nyob deb yuav tsum tseem ua tau raws li qhov kev txwv. Qhov no ob - rooj vag kaw lus (kub tawm tswv yim + chemistry) yog qhov muaj zog dua li kev cia siab rau cov khoom siv hluav taws xob ib leeg.

 

Qhov Kev Ntsuas Hardness Yuav Tsum Tau Ua API 6A Annex F Ntxiv Tshaj ASME IX?

 

API 6A Annex F ntxiv qhov yuav tsum tau kuaj xyuas qhov nyuaj rau ISO 15156-2 / NACE MR0175, uas tsis tas yuav tsum tau los ntawm ASME IX rau kev tsim nyog overlay ib leeg. Cov txheej txheem kev lees paub yog: lub hauv paus hlau thiab HAZ hardness Tsawg dua lossis sib npaug rau 250 HV (lossis Tsawg dua lossis sib npaug rau 22 HRC raws li cov xwm txheej tshwj xeeb), thiab overlay deposit hardness ib cov khoom specification. Qhov no yog qhov tseem ceeb tshaj plaws API 6A tshwj xeeb ntxiv rau kev tsim nyog overlay.

 

ASME IX tsis tas yuav tsum muaj kev sim hardness rau CRO kev tsim nyog. ASME IX xeem rau overlay yog: tshuaj ntsuam xyuas muaj pes tsawg leeg, kuaj khoov (4 sab khoov), thiab macro ntsuam xyuas. Hardness tsis nyob hauv QW-453.

 

API 6A, los ntawm kev siv rau ISO 15156-2, yuav tsum:Vickers hardness testing (HV10 lossis HV5) rau ISO 6507-1 / ASTM E92, tsawg kawg 12 qhov chaw sim hla peb txoj kev hla (pem hlau, HAZ, txhua txheej txheej). Rockwell hardness testing rau ISO 6508-1 / ASTM E-18 yog siv PWHT.

 

Kev lees txais raws li ISO 15156-2 / NACE MR0175:Base hlau thiab HAZ: Tsawg dua lossis sib npaug li 250 HV rau carbon, C-Mn, thiab qis- alloy steels. Yog tias tsim kev ntxhov siab tsawg dua lossis sib npaug ntawm 2/3 SMYS thiab PWHT suav nrog, Tsawg dua lossis sib npaug ntawm 22 HRC tuaj yeem siv hloov pauv. Cov nqi qis dua 20 HRC yuav tsum tau lees paub siv HRB nplai. Overlay deposit: raws li cov khoom specification.

 

Rau groove overlay (V-groove overlay applications), API 6A yuav tsum tau 3 hardness nyeem nyob rau hauv 3 hli ntawm lub hauv paus hlau ntawm weld cross-section, nrog nruab nrab Tsawg dua los yog sib npaug rau 92 HRBW.

 

Qhov kev ntsuas qhov hnyav no yog qhov laj thawj tseem ceeb vim li cas API 6A overlay kev tsim nyog muaj ntau dua thiab raug nqi ntau dua li ASME IX overlay kev tsim nyog. Nws ncaj qha hais txog cov kev pabcuam qaub tawg, uas ASME IX tsis ntsuas.

 

Dab tsi yog Khoov thiab Macro Examination Tests Yuav Tsum Tau?

 

Plaub qhov kev taw qhia -kev sim khoov thiab ib qho kev ntsuam xyuas macro ib PQR yuav tsum muaj rau kev tsim nyog tshaj ntawm ASME IX QW-453. API 6A txais yuav cov kev cai no thiab ntxiv LPT cov qauv kev lees paub rau ASME Tshooj V Tshooj 6.

 

What Bend and Macro Examination Tests Are Required

 

Khoov xeem:ASME IX QW-453 yuav tsum tau 4 qhov kev ntsuam xyuas sab-khoov (los yog 2 sab + 2 longitudinal sab khoov ua lwm txoj). Qhov kev lees paub: tsis muaj qhov qhib qhov tsis zoo tshaj 1.5 hli (1/16 nti) nyob rau hauv ib qho kev taw qhia, thiab tsis muaj qhov qhib qhov tsis zoo tshaj 3 hli (1/8 nti) hauv qhov chaw vuam. Cov khoov no sim cov kev sib raug zoo ntawm kev sib tshooj thiab lub hauv paus hlau.

 

Kev ntsuam xyuas Macro:Raws li ASME IX thiab ISO 15614-7, yam tsawg kawg 1 macro qauv ib PQR. Cov qauv yog etched rau ISO 17639 los qhia cov kab fusion, HAZ, thiab txheej txheej tsim. Kev lees txais: tsis muaj cov kab nrib pleb lossis kev tsis xws luag; tus kheej pores Tsawg dua los yog sib npaug li 2 hli; suab weld merging smoothly rau hauv lub hauv paus hlau rooj sib tham ISO 5817 Zoo Qib C; sau los ntawm cov duab ntawm ntau dua lossis sib npaug ntawm 5 × magnification.

 

API 6A LPT ntxiv:API 6A PSL 3 (Tshooj 7.5.2.2.9 thiab 7.5.2.3.8) yuav tsum tau kuaj cov kua dej nkag rau ntawm daim coupon tsim nyog overlay, ua tau raws li kev lees paub ntawm ASME Tshooj V Tshooj 6 / QW-195.2. Qhov LPT no tau ua tom qab PWHT thiab ua ntej kev kuaj kev puas tsuaj.

 

API 6A Annex F piv rau ASME IX QW-283 li cas rau Kev Tsim Nyog?

 

API 6A Annex F siv ASME IX QW-283 raws li lub hauv paus tseem ceeb ntawm cov txheej txheem sib txawv, tom qab ntawd ntxiv plaub txheej txheej tseem ceeb ntawm kev tswj: (1) yuav tsum tau kuaj ISO 15156 hardness, (2) tshuaj muaj pes tsawg leeg pov thawj khi rau overlay thickness nrug, (3) PSL-dependent NDE cov kev cai, thiab (4) kev sib xyaw ua ke ntawm cov hlau tshwj xeeb. Qhov tshwm sim yog ib qho kev tsim nyog uas yog nruj me ntsis kev saib xyuas dua li ASME IX ib leeg.

 

Cov lus hauv qab no qhia txog qhov sib txawv tseem ceeb:

 

Dimension

ASME IX QW-283

API 6A Annex F (+ Ntxiv)

Qhov tseem ceeb variables

QW-283.1 teev overlay-specific tseem ceeb variables rau ib tus txheej txheem

Tib qhov sib txawv ntawm ASME IX, ntxiv rau API 6A-Kev txwv tshwj xeeb ntawm chemistry thiab hardness

Kev Xeem Hardness

Tsis tas yuav tsum muaj CRO kev tsim nyog

Yuav tsum tau ua raws li ISO 15156-2 / NACE MR0175: HV / HRC kuaj hla 3 qhov kev hla, 12 qhov chaw tsawg kawg

Chemistry Verification

QW-453 Lus Cim 9: qauv ntawm overlay nto; nrug ntawm fusion kab=min. tsim nyog thickness

Tib txoj cai ASME IX, ntxiv rau API 6A Sec. 6.5.1.2.2: nrug yuav tsum tau sau tseg ntawm PQR; Fe cov ntsiab lus yuav tsum ua tau raws li qhov project spec (tsawg dua lossis sib npaug li 5% lossis tsawg dua lossis sib npaug li 10%)

Khoov Kev Xeem

4 sab khoov rau QW-453; max defect 1.5 hli / 3 hli

Tib yam kev cai ASME IX tau txais yuav

Kev xeem Macro

1 macro per PQR per QW-453; Daim ntawv pov thawj ISO 17639

Ib yam, ntxiv rau cov ntaub ntawv ntawm Ntau dua lossis sib npaug ntawm 5 × magnification rau ISO 15614-7

LPT ntawm daim coupon

Tsis xav tau rau overlay PQR

Yuav tsum tau rau PSL 3 rau API 6A Sec. 7.5.2.2.9; kev lees paub rau ASME V Art. 6

PWHT Variables

Kev hloov pauv tseem ceeb: hloov pauv hauv qhov xwm txheej lossis +25% sijhawm ntawm temp (A-Tsis yog. 9 nkaus xwb)

Tib txoj cai ASME IX; Ntxiv rau ISO 15156 hardness lees txais tom qab PWHT

Thaum tshav kub kub input (1st Layer)

+10% nce=kev hloov pauv tseem ceeb

Tib txoj cai ASME IX; ntxiv rau chemistry pov thawj raws li kev kuaj thib ob

Kev xaiv khoom siv

Rau A-Number / F-Kev faib tus lej; lub npe lag luam kaw yog tias tsis yog - tus qauv

Ib yam, ntxiv rau API 6A Sec. 5.4 tsuas yog teev cov qauv siv tau tshwj xeeb

Overlay Thickness Ntsuas

Tsis tau teev nyob rau hauv ASME IX rau kev ntsuas ntau lawm

Chaw tsim tshuaj paus cov lus qhia tshwj xeeb yuav tsum suav nrog cov txheej txheem ntsuas qhov tuab (PSL 2/3/4)

 

Cov lus: Kev sib piv ntawm cov kev cai overlay tsim nyog ntawm ASME IX QW-283 thiab API 6A Annex F. Blue-shaded kab qhia txog qhov cuam tshuam tshaj plaws API 6A ntxiv.

 

Dab tsi yog qhov kev cuam tshuam rau cov neeg tsim khoom?

 

Cov neeg tsim khoom yuav tsum tau nqis peev rau hauv cov txheej txheem, ntau- qhov kev tsim nyog tau txais txiaj ntsig sib txawv uas hais txog ASME IX thiab API 6A cov kev cai ib txhij. Cov tswv yim tseem ceeb suav nrog: tsim nyog ntawm cov khoom siv hauv paus, xaiv qis- cov txheej txheem dilution, sau ua ntej- txheej txheej tsis muaj qhov siab, thiab tsim PQR daim coupon xeem kom npog cov txheej txheem ntau lawm overlay thickness.

 

1. Cov tswv yim tsim nyog:Hloov chaw tsim nyog overlay ntawm txhua qib hlau hauv ib tus neeg, cov tuam txhab lag luam yuav tsum tsom rau P-Cov pab pawg uas suav nrog feem ntau ntawm lawv cov khoom lag luam zoo (P-Tsis yog. 1} rau A105/A106, P{{5}Tsis yog. 4/5A rau F22/F11, ntxiv rau cov ntaub ntawv tsis raug xaiv los ntawm AI74).

 

2. Txheej txheem xaiv:Automated GTAW nrog pulsed kub- hlau yog cov txheej txheem pom zoo rau API 6A overlay ntau lawm. Nws qhov qis qis (feem ntau Tsawg dua lossis sib npaug li 10%) ua rau nws yooj yim dua kom ua tau raws li Fe Tsawg dua lossis sib npaug li 5% ntawm cov kab sib txuas uas tau teev tseg, thiab nws qhov kev ntsuas kev taug qab txhawb nqa PSL 3/4 kev soj ntsuam cov cai.

 

3. PQR daim coupon tsim:Qhov kev xeem daim coupon overlay thickness yuav tsum yog tsawg kawg yog 5 hli kom tsim nyog ntau lawm overlays mus txog 7.5 hli (1.5 × txoj cai). Cov qauv chemistry yuav tsum tau coj mus rau qhov project qhov tsawg kawg nkaus overlay thickness nrug (feem ntau 3 hli los ntawm fusion kab rau Alloy 625).

 

4. Kev tswj hwm kev hloov pauv hloov pauv:Txhua qhov kev thov hloov mus rau qhov hloov pauv tseem ceeb yuav tsum tau soj ntsuam ua ntej tsim khoom. Yog tias qhov kev hloov pauv ntau dhau qhov tsim nyog, kev tsim nyog yuav tsum tau ua. Tej yam tshwm sim: ntau hom muab tub lim (yog tias tsis yog - tus qauv), nce PWHT lub sij hawm, dav txoj hauj lwm ntau, siab dua ua ntej - txheej cua sov nkag.

 

5. Kev qhuab qhia cov ntaub ntawv:Sau tag nrho cov kev sib txuas tiag tiag ntawm PQR nrog qhov tseeb tag nrho (V, A, kev mus ncig ceev, cov khoom siv hluav taws xob hauv ib txheej, preheat / interpass kub, PWHT kub thiab sijhawm). Cov ntaub ntawv no txhais tau qhov tsim nyog ntau yam thiab yuav raug tshuaj xyuas raws li API 6A PSL 3/4 cov cai.

 

Dab tsi yuam kev ua rau Overlay Kev Tsim Nyog Tsis Ua Haujlwm?

 

Peb feem ntau ua rau overlay qualification tsis ua hauj lwm yog: (1) ntau dhau dilution ua rau Fe cov ntsiab lus siab tshaj qhov kev txwv, (2) HAZ hardness tshaj 250 HV / 22 HRC, thiab (3) khoov kev xeem tsis xws luag ntawm fusion kab qhia tias tsis zoo daim ntawv cog lus. Tag nrho peb qhov no tsuas yog kuaj tau los ntawm API 6A- cov kev sim tshwj xeeb (kev tshuaj xyuas tshuaj lom neeg thiab kev sim hardness) uas dhau mus dhau ASME IX.

 

Kev siv ntau dhau (Fe> 5% lossis> 10%):Ua los ntawm ib yam nkaus thiab- cov cua kub nkag rau thawj txheej, cov hlaws tsis zoo sib tshooj, lossis siv cov txheej txheem siab - dilution (xws li, phau ntawv SMAW) tsis muaj cov txheej txheem txaus. Kev kho: hloov mus rau qis-dilution GTAW, ua kom zoo dua ua ntej- txheej txheej, lossis ntxiv txheej tsis.

 

HAZ hardness> 250HV:Ua los ntawm qhov tsis txaus preheat, kub interpass ntau dhau, tsis txaus PWHT, los yog siv lub substrate uas muaj zog hardenability (xws li, AISI 4130) tsis muaj thermal tswj. Kev kho: nce preheat, tswj qhov kub thiab txias, siv PWHT tsim nyog rau ISO 15156-2.

 

Khoov xeem fusion- kab tsis xws luag:Qhib qhov tsis xws luag ntawm overlay/base hlau interface thaum lub sij hawm sab- khoov kuaj, qhia tias tsis tiav fusion los yog tsis muaj zog daim ntawv cog lus. Kev kho: txheeb xyuas qhov huv ntawm qhov chaw ua ntej overlay, ua kom zoo dua ua ntej - txheej arc yam ntxwv, thiab xyuas kom muaj kev tiv thaiv roj kom zoo.

 

Cov ntaub ntawv tsis tiav:PQR ploj lawm qhov chemistry sampling nrug, ua ntej -layer heat input xam, los yog hardness traverse data. Qhov no tsis yog qhov kev sim ua tsis tiav, tab sis nws ua tsis tau raws li PQR rau API 6A lub hom phiaj thiab yuav tsum tau rov ua dua -cov ntaub ntawv lossis rov- kuaj.

 

Xaus

 

Weld overlay kev tsim nyog raws li API 6A Annex F yog ntau -qhov kev ua raws li kev ua raws li cov txheej txheem ISO 15156 hardness tswj thiab chemistry pov thawj cov cai nyob rau sab saum toj ntawm ASME Tshooj IX QW-283 qhov tseem ceeb ntawm cov txheej txheem sib txawv. Qhov tseem ceeb variables - txheej txheem vuam, cov khoom siv hauv paus P-Number, muab tub lim hlau A/F-Number, overlay thickness, vuam txoj hauj lwm, preheat/interpass kub, PWHT tej yam kev mob, thiab thawj- txheej thaum tshav kub kub input - txhais lub hnab ntawv tsim nyog. Ib qho kev hloov pauv sab nraum lub hnab ntawv no yuav tsum muaj kev tsim nyog tag nrho.

 

Rau cov chaw tsim khoom ntawm stainless hlau thiab npib tsib xee alloy wellhead cov cuab yeej, qhov tseem ceeb ntawm cov khoom siv yog: API 6A Annex F kev tsim nyog yog nruj me ntsis xav tau tshaj li ASME IX ib leeg. ISO 15156 hardness testing thiab chemistry verification ntawm fusion kab nrug yog ob lub rooj vag uas feem ntau ntes cov txheej txheem uas yuav dhau ASME IX tab sis ua tsis tau raws li API 6A. Tsim cov txheej txheem overlay kom dhau cov rooj vag no los ntawm thawj PQR sim - los ntawm kev xaiv qis - cov txheej txheem dilution, tswj ua ntej - txheej txheej cua sov input kom meej, thiab siv cov PWHT - kom txuag lub sij hawm, nqi, thiab kev tswj kev pheej hmoo.

 

 