Khoov thiab tsim Duplex Yeeb Nkab Kev Ceeb Toom thiab Tsawg Radius

Jun 26, 2026

Tso lus

Duplex stainless hlauua ke lub zog siab ntawm qib ferritic nrog rau corrosion kuj thiab toughness ntawm qib austenitic. Qhov kev sib xyaw tshwj xeeb no ua rau lawv zoo tagnrho rau kev thov hauv cov roj thiab roj, kev ua tshuaj lom neeg, desalination, thiab offshore platforms. Txawm li cas los xij, tib lub dual -theem microstructure uas muab duplex nws qhov zoo kuj tsim cov kev sib tw thaum khoov thiab ua haujlwm.

 

Tsis zoo li austenitic stainless hlau, uas yog cov ductile heev thiab zam txim, cov qib duplex muaj qhov txwv ntau dua. Cov theem ferrite muaj zog dua tab sis tsawg dua ductile tshaj li theem austenite. Thaum lub caij txias txias, qhov sib txawv ntawm lub zog no tuaj yeem ua rau tsis yog -ib puag ncig deformation, ntau lub caij nplooj ntoos hlav rov qab, thiab nyob rau hauv cov xwm txheej hnyav, tawg hauv qhov nro ntawm qhov khoov.

 

Bending and Forming Duplex Pipe Precautions and Minimum Radius

 

Tsab ntawv xov xwm no muab cov lus qhia tswv yim rau kev khoov thiab tsim duplex stainless hlau yeeb nkab. Nws suav nrog qhov yuav tsum tau khoov tsawg kawg nkaus, txias vs. kub dabtsi yog khoov kev txiav txim siab, cov nyiaj them rov qab, thiab cov kev ceev faj tseem ceeb uas yuav tsum tau ua kom muaj kev tiv thaiv corrosion thiab cov khoom siv kho tshuab tom qab tsim.

 

Mechanical Properties

 
Lub zog muaj zog ntau dua thiab kev ua haujlwm tsis muaj zog hauv duplex steels yuav tsum tau khoov radii loj dua thiab cov nyiaj them rov qab ntau dua li cov qib austenitic
 

Cov khoom siv ntawm duplex stainless hlau sib txawv ntawm cov qib austenitic. Kev nkag siab txog qhov sib txawv no yog qhov tseem ceeb rau kev ua haujlwm khoov kom zoo.

 

Table 1: Mechanical Properties Comparison for Bending Behavior

Khoom

Austenitic (304L)

Duplex (2205)

Super -Duplex (2507)

Qhov cuam tshuam rau Bending

Yield zog

170-200 MPa

450-550 MPa

550-650 MPa

Yuav tsum muaj zog dua

Tensile zog

485-515 MPa

620-750 MPa

795-900 MPa

Ntau resistant rau deformation

Elongation

40-50%

25-35%

15-25%

Tsawg ductility margin

Ua Haujlwm Hardening Rate

Siab

Nruab nrab

Tsawg- Nruab nrab

Tsawg zog thaum khoov

Springback

Tsawg- Nruab nrab

Siab

Siab heev

Yuav tsum tau them nyiaj

Tau qhov twg los: ASTM A240 / A240M-24; Outokumpu Duplex Stainless Hlau Phau Ntawv (2015); Sandvik SAF 2205/2507 Daim Ntawv Teev Npe

 

Lub zog ntawm duplex 2205 yog kwv yees li 2.5 npaug ntawm 304L austenitic stainless hlau. Lub zog siab dua no txhais tau hais tias kev khoov duplex yeeb nkab yuav tsum tau muaj zog ntau dua thiab ua rau muaj kev rov zoo dua qub (caij nplooj ntoos hlav) tom qab lub bending load raug tshem tawm. Tus neeg tsim khoom yuav tsum suav rau lub caij nplooj ntoo hlav no los ntawm ntau dua - khoov lossis los ntawm kev siv cov cuab yeej khoov precision nrog cov nyiaj them rov qab.

 

Yam tsawg kawg nkaus Khoov Radius rau Cold Bending: Tus Qauv Kev Lag Luam

 
Rau txias dabtsi yog khoov ntawm duplex yeeb nkab, qhov tsawg kawg nkaus khoov vojvoog yuav tsum yog 4-5 npaug ntawm sab nraud txoj kab uas hla (D), piv rau 2-3D rau austenitic qib
 

Qhov tsawg kawg nkaus khoov vojvoog yog lub vojvoog me tshaj plaws nyob ib puag ncig uas cov yeeb nkab tuaj yeem khoov tau yam tsis ua rau qhov tsis tuaj yeem deformation, phab ntsa thinning, lossis tawg. Rau duplex stainless hlau, qhov tsawg kawg nkaus khoov vojvoog yog loj dua rau cov qib austenitic vim lub zog siab dua thiab qis dua ductility ntawm ferrite theem.

 

Table 2: Yam tsawg kawg Cold Khoov Radius los ntawm cov yeeb nkab loj thiab cov khoom siv

Pipe Size (OD)

Austenitic (304/316) Min Radius

Duplex (2205) Min Radius

Super-Duplex (2507) Min Radius

Qhov siab tshaj plaws ovality

Mus txog 2 nti (50 mm)

2D - 3D

4D - 5D

5D - 6D

5-8%

2-6 nti (50-150mm)

3D - 4D

5D - 6D

6D - 7D

5-8%

6-12 nti (150-300mm)

4D - 5D

6D - 7D

7D - 8D

6-9%

12-24 nti (300-600mm)

5D - 6D

7D - 8D

8D - 10D

6-10%

Above 24 inch (>600 hli)

6D - 8D

8D - 10D

10D - 12D

8-12%

Tau qhov twg los: ASME B31.3 Txheej Piping (2022); ASTM A999 / A999M-24; Outokumpu Cov Lus Qhia Ua Haujlwm; Sandvik Yeeb Nkab Khoov Cov Lus Qhia

 

Qhov piv ntawm khoov vojvoog rau cov yeeb nkab txoj kab uas hla (R / D) yog tus qauv parameter rau kev qhia khoov. Ib qho 5D khoov ntawm 6-nti yeeb nkab muaj qhov nkhaus ntawm 30 ntiv tes (5 x 6). Tighter khoov (me me R / D ratios) yog ua tau nrog kub dabtsi yog khoov los yog nrog cov khoom tshwj xeeb, tab sis lawv ua rau muaj kev pheej hmoo ntawm phab ntsa thinning, ovality, thiab microstructural puas.

 

Txias dabtsi yog khoov: txheej txheem tswj thiab txwv

 
Txias dabtsi yog khoov tau rau duplex yeeb nkab mus txog kwv yees li 12-inch inch nrog cov khoom tsim nyog, lubrication, thiab xuab zeb los yog mandrel txhawb
 
Bending and Forming Duplex Pipe Cold Bending
 

Txias dabtsi yog khoov yog hais txog kev tsim cov haujlwm ua haujlwm ntawm chav tsev kub yam tsis muaj cua sov sab nraud. Nws yog txoj hauv kev zoo tshaj plaws rau cov yeeb nkab dabtsi yog khoov hauv cov khw muag khoom vim tias nws yuav tsum tau siv cov cuab yeej tshwj xeeb tsawg dua thiab nrawm dua li kub dabtsi yog khoov. Txawm li cas los xij, txias khoov muaj kev txwv rau duplex stainless hlau.

 

Phab ntsa thinning: Sab phab ntsa ntawm qhov khoov (extrados) stretches thiab thins thaum khoov. Rau cov qib duplex, phab ntsa thinning yuav tsum tau txwv rau 12-15% ntawm nominal phab ntsa thickness kom muaj siab ncaj ncees.

 

Ovality: Cov yeeb nkab hla- ntu zoo li flatten thaum lub sij hawm khoov, tsim cov duab oval. Rau duplex yeeb nkab, ovality yuav tsum tau txwv rau 8% siab tshaj, xam raws li (Dmax - Dmin) / Davg x 100%.

 

Wrinkling: Sab hauv phab ntsa ntawm qhov khoov (intrados) yog nyob rau hauv compression thiab yuav wrinkle yog tias cov phab ntsa thickness tsis txaus lossis yog tias txoj kev khoov tsis muab kev txhawb nqa txaus. Kev them nyiaj yug sab hauv (xuab zeb sau, mandrel, lossis hloov tau yooj yim) yog qhov tseem ceeb rau nyias -cov yeeb nkab phab ntsa.

 

Springback: Duplex steels nthuav tawm qhov tseem ceeb springback vim lawv lub zog tawm los siab. Tus neeg tsim khoom yuav tsum dhau - khoov los ntawm tus nqi tsim nyog kom ua tiav lub kaum sab xis kawg. Springback them ntawm 5-15 degrees yog ib qho zoo rau duplex, piv rau 2-8 degrees rau qib austenitic.

 

Table 3: Txias Bending Parameters thiab tswj txoj kev

Bending Parameter

Austenitic SS

Duplex (2205)

Super -Duplex (2507)

Tswj Txoj Kev

Max Phab ntsa Thinning

12-15%

10-12%

8-10%

Ultrasonic ntsuas

Max Ovality

8-10%

6-8%

5-7%

Caliper ntsuas

Springback Angle

2-8 degrees

5-15 degrees

10-20 degrees

Kev sim khoov, dhau -khoov

Min Phab ntsa rau Tight Khoov

Teem caij 40

Teem caij 80

Teem caij 80/160

Kev txiav txim siab tsim

Kev them nyiaj yug sab hauv

Pom zoo

Yuav tsum tau

Yuav tsum tau

Xuab zeb, mandrel, los yog muab tub lim

Source: ASME B31.3 (2022); PFI ES-24 Pipe Bending Methods; Outokumpu Fabrication Guidelines

 

Kub dabtsi yog khoov: Thaum twg thiab yuav ua li cas thov kub

 
Kub dabtsi yog khoov ntawm 950-1100 C tso cai nruj dua radii (2-3D) rau duplex yeeb nkab tab sis yuav tsum tau muab tshuaj annealing tom qab los kho corrosion kuj.
 

Kub dabtsi yog khoov muaj cua sov cov yeeb nkab kom siab kub ua ntej sib sau. Lub tshav kub txo lub zog tawm los thiab nce ductility, tso cai rau kev khoov nruj dua nrog kev tsim quab yuam tsawg thiab txo qis springback. Txawm li cas los xij, kub dabtsi yog khoov ntawm duplex stainless hlau qhia txog metallurgical txaus ntshai uas yuav tsum tau ua tib zoo tswj.

 

Qhov tseem ceeb xav txog yog qhov kub thiab txias. Cua sov duplex stainless hlau mus rau hauv 600-900 degrees Celsius ntau yam txhawb kev tsim ntawm sigma theem thiab lwm yam intermetallic tebchaw, uas heev txo corrosion kuj thiab toughness. Qhov no yog tib yam rhiab heev mechanism sib tham nyob rau hauv welding, thiab nws siv sib npaug rau kub sib sau ua hauj lwm.

 

Kev nyab xeeb kub dabtsi yog khoov xyaum yuav tsum tau:

 

Ua kom sov cov yeeb nkab rau 950-1100 degrees Celsius (siab dua qhov kub ntawm sigma solvus) ua ntej khoov. Siv cov ntsuas kub-qhia cov crayons lossis pyrometers los txheeb xyuas.

 

Ua kom tiav qhov kev ua haujlwm khoov sai sai thaum cov khoom nyob ntawm qhov kub thiab txias. Tsis txhob so ntev ntawm qhov kub nruab nrab.

 

Cov tshuaj anneal tam sim ntawd tom qab khoov ntawm 1020-1100 degrees Celsius, ua raws li los ntawm kev txias sai (dej quench los yog yuam cua). Qhov no dissolves ib theem sigma uas tej zaum yuav tau tsim thiab restores qhov tseeb theem tshuav nyiaj li cas.

 

Document lub voj voog thermal. Rau cov ntawv thov tseem ceeb, khaws cov ntaub ntawv ntawm lub sijhawm cua sov, qhov kub thiab txias, thiab txoj kev ua kom txias kom zoo.

 

Table 4: Kub dabtsi yog khoov kub Parameters rau Duplex Stainless hlau

Parameter

Pom zoo Range

Tseem ceeb txwv

Qhov tshwm sim ntawm kev ua txhaum cai

Preheat kub

950-1100 C

Tsis txhob siab tshaj 1150 C

Kev loj hlob qoob loo ntau dhau

Sijhawm ntawm Kub

Tsawg (5-15 feeb ib txwm)

Tsis txhob ncua kev tuav pov hwm

Nto oxidation, scaling

Forbidden Temperature Range

N/A

600-900 C

Sigma theem tsim

Tshaj tawm -Bend Solution Anneal

1020-1100 C

Yuav tsum tau kub khoov

Corrosion kuj poob

Txoj kev txias

Dej quench los yog cua ceev

Tsis txhob maj txias

Sigma re- nag lossis daus

Tau qhov twg los: Outokumpu Cov Txheej Txheem Kub Ua Haujlwm; ASTM A999 / A999M-24; NACE MR0175/ISO 15156; Sandvik Cov lus pom zoo kho cua sov

 

Springback Compensation: Predicting thiab Kho Elastic Recovery

 
Duplex yeeb nkab nthuav tawm 2-3 zaug ntxiv springback dua qib austenitic; kev them nyiaj yuav tsum tau txiav txim siab empirically rau txhua cov yeeb nkab loj thiab phab ntsa thickness
 
Predicting and Correcting Elastic Recovery
 

Springback yog qhov elastic rov qab uas tshwm sim thaum lub bending load raug tshem tawm. Cov yeeb nkab khoov 'caij rov qab' mus rau nws cov duab qub, uas ua rau lub kaum sab xis kawg me dua lub kaum sab xis ua tiav thaum lub sijhawm tsim. Tus nqi ntawm springback nyob ntawm qhov tawm los lub zog, elastic modulus, khoov vojvoog, thiab cov yeeb nkab geometry.

 

Rau duplex stainless steels, lub siab yield zog ua rau muaj zog springback ntau dua austenitic qib. Ib txoj cai ntawm tus ntiv tes xoo yog tias duplex springback yog kwv yees li 2-3 npaug ntawm 304L lossis 316L rau tib lub geometry. Qhov no yuav tsum tau them rov qab los ntawm kev khoov dhau los yog siv cov cuab yeej siv nrog lub caij nplooj ntoos hlav twv ua ntej algorithms.

 

Table 5: Springback Comparison thiab Over-Bend Requirements

Tube OD x Phab ntsa

Khoov Radius

Austenitic Springback

Duplex (2205) Springback

Tshaj -Yuav tsum tau khoov

2cm40 ib

3D

2-4 degrees

5-8 degrees

+6-10 degrees

4 px40

4D

3-5 degrees

7-12 degrees

+8-15 degrees

6 nc80

5D

4-6 degrees

10-15 degrees

+12-18 degrees

8 nc80

6D

5-8 degrees

12-18 ° C

+15-22 degrees

12 nti Sch80

7D

6-10 degrees

15-25 ° C

+18-30 degrees

Source: PFI ES-24; Cov ntaub ntawv tsim tawm los ntawm JN Alloys; Kev coj ua zoo tshaj plaws hauv kev lag luam

 

Cov nqi hauv Table 5 yog cov lus qhia. Qhov tseeb springback txawv nrog cov khoom siv hluav taws xob tshwj xeeb, lub vojvoog khoov tseeb, thiab txoj kev khoov. Rau cov ntawv thov tseem ceeb, ua qhov kev sim khoov ntawm cov qauv ntu kom txiav txim siab lub caij nplooj ntoos hlav caij nplooj ntoos hlav, tom qab ntawd kho qhov khoov teeb raws li.

 

Txoj kev tsim: Rotary Draw, Compression, thiab Roll Bending

 
Rotary kos dabtsi yog khoov nrog kev txhawb nqa sab hauv mandrel muab kev tswj zoo tshaj plaws rau nruj -radius duplex yeeb nkab khoov
 

Ob peb txoj kev yog siv rau dabtsi yog khoov yeeb nkab, txhua tus muaj qhov zoo thiab kev txwv rau duplex stainless hlau:

 

Rotary kos dabtsi yog khoov: Cov yeeb nkab yog clamped thiab kos nyob ib ncig ntawm ib tug rotating tuag. Txoj kev no muab kev tswj zoo tshaj plaws ntawm khoov geometry thiab yog txoj kev nyiam rau kev nruj- vojvoog khoov. Internal mandrel txhawb tiv thaiv kev sib tsoo thiab txo ovality. Qhov tseem ceeb rau cov yeeb nkab duplex nrog R / D tsawg dua 5.

 

Compression dabtsi yog khoov: Cov yeeb nkab yog tuav ruaj khov thaum lub menyuam los yog khau presses tiv thaiv nws los tsim khoov. Cov cuab yeej siv yooj yim tab sis tswj tsawg dua geometry. Haum rau cov kab hluav taws xob loj dua (6D thiab siab dua) qhov twg ovality tsis tshua muaj teeb meem.

 

Yob dabtsi yog khoov (3- yob los yog 4-yob): Cov yeeb nkab hla dhau ib txheej ntawm cov chais uas maj mam tsim qhov nkhaus. Siv rau loj-radius khoov thiab tsim arcs los yog coils. Muab cov curvature zoo ib yam tab sis kev tswj tsis pub dhau lub kaum sab xis. Txais tau rau duplex thaum khoov vojvoog yog 8D lossis ntau dua.

 

Induction dabtsi yog khoov: Ib cheeb tsam cua sov yog tsim los ntawm electromagnetic induction thaum cov yeeb nkab raug thawb los ntawm ib sab caj npab. Muab qhov zoo ntawm kev khoov kub nrog kev tswj xyuas meej. Feem ntau rau - txoj kab uas hla cov yeeb nkab (12 nti thiab siab dua) hauv kev siv roj thiab roj. Yuav tsum tau ceev faj tswj qhov kub thiab txias tom qab- khoov kub.

 

Table 6: Khoov txoj kev xaiv rau Duplex Stainless Hlau Yeeb Nkab

Txoj kev khoov

Puas tsim nyog rau Duplex?

Min Khoov Radius

Daim ntawv thov zoo tshaj plaws

Kev txiav txim siab tseem ceeb

Rotary Draw nrog Mandrel

Yog - Nyiam

3D - 4D

Tight khoov, precision ua haujlwm

Mandrel xaiv qhov tseem ceeb

Rotary Draw w/o Mandrel

Kev siv tsawg

5D - 6D

Thick -cov yeeb nkab

Saib rau ovality

Compression dabtsi yog khoov

Txais tau

6D - 8D

Field fabrication

Tsawg qhov tseeb tshaj rotary

Roll Bending

Txais tau

8D - 10D

Loj radius, coils

Yuav tsum muaj ntau daim ntawv hla tebchaws

Induction Bending

Yog - Rau OD loj

3D - 5D

Loj txoj kab uas hla

Tshaj tawm - khoov tshuaj anneal

Tau qhov twg los: PFI ES-24 Pipe Bending Methods; ASME B31.3; JN Alloys Fabrication Experience

 

Kev soj ntsuam zoo tom qab khoov: Yuav kuaj li cas

 
Tom qab- khoov tshuaj xyuas yuav tsum xyuas kom meej phab ntsa thickness, ovality, deg mob, thiab rau kub khoov, theem sib npaug thiab corrosion kuj
 

Kev tshuaj xyuas zoo tom qab khoov yog qhov tseem ceeb los xyuas kom meej tias cov yeeb nkab ua tau raws li cov qauv tsim thiab tsis muaj kev puas tsuaj thaum lub sij hawm tsim. Qhov kev tshuaj ntsuam xyuas nyob ntawm qhov tseem ceeb ntawm daim ntawv thov thiab seb qhov kub thiab txias dabtsi yog siv.

 

Duplex Pipe Quality Inspection After Bending

 

Phab ntsa thickness ntsuas: Siv ultrasonic ntsuas los ntsuas phab ntsa thickness ntawm lub extrados (sab khoov), intrados ( puab khoov), thiab nruab nrab axis. Muab piv rau qhov tsawg kawg nkaus tsim thickness. Pom tau thinning feem ntau yog 10-12% rau duplex, nrog rau cov extrados yog qhov chaw tseem ceeb.

 

Kev ntsuas ovality: Ntsuas qhov siab tshaj plaws thiab qhov tsawg kawg nkaus txoj kab uas hla hauv cheeb tsam khoov. Muab xam ovality li (Dmax - Dmin) / Davg x 100%. Rau duplex, cov qauv kev lees paub yog 6-8% siab tshaj plaws.

 

Kev soj ntsuam saum npoo: Tshawb xyuas cov npoo sab nrauv thiab sab hauv kom pom cov kab nrib pleb, khawb, khawb, lossis kab mob. Duplex stainless hlau muaj qhov cuam tshuam rau kev ntxhov siab corrosion tawg yog tias qhov chaw puas hauv kev pabcuam, yog li kev tiv thaiv nto thaum tuav yog qhov tseem ceeb.

 

Khoov lub kaum sab xis pov thawj: Ntsuas qhov kawg khoov lub kaum sab xis thiab muab piv rau qhov tsim nyog yuav tsum tau ua. Tus account rau ib qho kev tolerance uas teev nyob rau hauv engineering tsim.

 

Theem nyiaj tshuav (kub khoov nkaus xwb): Rau kub-khoov duplex yeeb nkab, ferrite ntsuas los ntawm cov cuab yeej sib nqus los yog kev kuaj xyuas metallographic paub meej tias cov theem sib npaug yog nyob rau hauv qhov tau txais (feem ntau 35-65% ferrite). Tawm ntawm - ntawm-spec theem tshuav nyiaj li cas qhia tias kev kho cua sov tsis raug.

 

Kev kuaj Corrosion (cov ntawv thov tseem ceeb): Rau qhov chaw pabcuam hnyav, kev kuaj corrosion (pitting kuj, intergranular corrosion) ntawm cov qauv los ntawm khoov cheeb tsam yuav raug teev los xyuas kom meej tias cov kev ua haujlwm tsis cuam tshuam rau corrosion.

 

Table 7: Tshaj tawm -Kov Kev Tshawb Fawb Yuav Tsum Tau Ua rau Duplex Yeeb Nkab

Cov khoom soj ntsuam

Txoj kev

Kev lees txais

Ntau zaus

Phab ntsa Thickness

Ultrasonic

Min 88% ntawm nominal (tus qauv)

Txhua khoov

Ovality

Caliper / Template

Max 6-8% (tus qauv)

Txhua khoov

Surface condition

Visual / Dye Penetrant

Tsis muaj kab nrib pleb, khawb tob

100% pom, PT raws li tau teev tseg

Khoov lub kaum sab xis

Protractor / CMM

Raws li tus qauv kam rau ua (+/- 0.5-1 deg raug)

Txhua khoov

Cov ntsiab lus Ferrite

Sib nqus ntsuas

35-65% (kub khoov)

Qauv los yog txhua qhov khoov

Corrosion Test

ASTM G48 / A262

Raws li specification

Qauv los yog raws li tau teev tseg

Source: ASME B31.3; ASTM A999 / A999M-24; ASTM G48-11; ASTM A262-15; NWS MR0175

 

Xaus

 

Bending duplex stainless hlau yeeb nkab yuav tsum tau ua tib zoo saib xyuas cov txheej txheem tswj dua li khoov qib austenitic. Lub zog tawm los ntau dua, txwv tsis pub ductility, thiab rhiab heev rau kev tsim cov theem sigma tag nrho ua rau lub qhov rais nqaim dua. Txawm li cas los xij, nrog kev nkag siab zoo ntawm cov khoom coj tus cwj pwm thiab cov cuab yeej tsim nyog, cov yeeb nkab duplex tuaj yeem tsim kev ntseeg siab rau kev thov kev pabcuam.

 

Cov ntsiab cai tseem ceeb yog:

 

Siv qhov khoov radii loj (4-5D yam tsawg kawg nkaus) rau kev khoov txias kom tiv thaiv kev tawg thiab tawg ntau dhau.

 

Ib txwm muab kev txhawb nqa sab hauv (mandrel lossis xuab zeb) los tswj ovality thiab tiv thaiv wrinkling.

 

Tus account rau qhov tseem ceeb springback (2-3 npaug ntawm cov qib austenitic) los ntawm kev khoov dhau.

 

Yog xav tau kub dabtsi yog khoov, kub siab tshaj 950 C thiab ib txwm ua raws li kev daws teeb meem annealing.

 

Tshawb xyuas phab ntsa tuab, ovality, thiab qhov chaw saum npoo tom qab khoov; rau kub khoov, xyuas cov theem sib npaug.

 

Sau cov txheej txheem khoov rau cov ntawv thov tseem ceeb kom ntseeg tau tias muaj kev taug qab.

 

Rau kev txhawb nqa ntawm duplex stainless hlau yeeb nkab specifications, tsim cov txheej txheem, los yog xaiv cov ntaub ntawv, hu rau JN Alloys -- koj tus khub nyob rau hauv high-kev ua tau zoo alloy kev daws teeb meem.

 

Lub Vev Xaib:www.jnalloys.com

 

Xa kev nug
Los rau peb
Thiab pib koj rfqs tam sim no.
Tiv Tauj Peb