321 Stainless Steel Creep Cov Ntaub Ntawv: Ntev-Lub Sij Hawm Siab- Kev Ua Haujlwm Kub Kub hauv Kev Pabcuam Refinery

Aug 24, 2026

Tso lus

Refineries ua haujlwm qee qhov xav tau siab tshaj - cov khoom siv kub hauv kev lag luam. Cov raj cua sov, cov kav dej hloov kho, thiab cov khoom siv hluav taws xob ua rau pom qhov kub ntawm 425 thiab 870 degrees C. Nyob rau hauv cov xwm txheej no, xaiv cov khoom siv tsis raug tsis yog ib qho teeb meem ntawm kev txo qis kev ua haujlwm - nws yog ib qho teeb meem ntawm kev nyab xeeb, kev ua raws cai, thiab ntau - lab -$ cov cuab yeej siv tau ntev.

 

321 Stainless Steel Creep Data

 

321 stainless hlau(UNS S32100)yog titanium-stabilized austenitic qib tshwj xeeb tsim los tiv thaiv intergranular corrosion thiab tuav lub zog creep nyob rau hauv qhov kub thiab txias qhov twg tus qauv 304 stainless hlau tsis ua hauj lwm. Kab lus no nthuav tawm cov ntaub ntawv sib sau ua ke ntawm 321 stainless hlau creep - nrog rau kev ntxhov siab rupture zog, 1% creep txwv, ASME tso cai rau kev ntxhov siab, thiab kev sib piv kev ua tau zoo - los pab engineers thiab procurement managers txiav txim siab cov ntaub ntawv rau lub sij hawm ntev - refinery kev pab cuam.

 

Ntsiab Cai

 

321 stainless hlau (UNS S32100) yog titanium - ruaj khov rau kev pabcuam hauv 425-900 degrees C ntau yam, tiv thaiv intergranular corrosion hauv welded refinery Cheebtsam.

 

100,000-teev creep rupture zog: kwv yees li 90 MPa ntawm 600 degrees C thiab 50 MPa ntawm 650 degrees C - txaus rau 20 xyoo refinery tsim lub neej.

 

ASME Tshooj II-D (2023) tso cai rau kev ntxhov siab rau 321: 117 MPa ntawm 500 ° C, 52 MPa ntawm 600 ° C, thiab 18 MPa ntawm 700 ° C.

 

321 outperforms 304 los ntawm 15-25% nyob rau hauv creep rupture zog thiab yog piv rau 347 hauv qab 650 degrees C.

 

Hloov kho mus rau 321H (cov pa roj carbon ntau dua, cov nplej ntxhib) thaum ua haujlwm siab tshaj 538 degrees C nyob rau hauv kev ua haujlwm ruaj khov.

 

Dab tsi yog 321 Stainless Hlau thiab Vim Li Cas Nws Stabilized nrog Titanium?

 

321 stainless hlau yog titanium-stabilized austenitic chromium-nickel stainless hlau (UNS S32100, EN 1.4541) engineered los tiv thaiv intergranular corrosion nyob rau hauv 425-900 degrees C ntau yam, ua rau nws cov qib zoo dua rau cov khoom siv welded.

 

Chemical Composition thiab Stabilization Mechanism.321 belongs to the 18-8 austenitic family - the same base composition as 304 stainless steel - but with a critical addition: titanium. The titanium content must be at least five times the carbon content (Ti >= 5xC) kom ua tiav qhov ruaj khov. Qhov kev xav tau no tau teev tseg hauv ASTM A276, ASTM A479, thiab ASTM A240 tus qauv.

 

Nyob rau hauv tus qauv 304 stainless hlau, ntev raug rau qhov kub thiab txias ntawm 425 thiab 815 degrees C ua rau chromium carbides (Cr23C6) rau precipitate ntawm grain ciam teb. Qhov no depletes chromium los ntawm cov hlau ib puag ncig, tsim cov cheeb tsam yooj yim rau intergranular corrosion. Nyob rau hauv 321, titanium nyiam khi nrog carbon los tsim titanium carbides (TiC) faib randomly thoob plaws hauv cov nplej - tsis nyob rau hauv ciam teb. Cov chromium tseem nyob hauv kev daws, thiab cov txheej txheem oxide passive nyob twj ywm.

 

Kev Siv Tau.Qhov kev ruaj khov no yog vim li cas 321 tuaj yeem welded thiab muab tso rau hauv kev pabcuam hauv carbide nag lossis daus yam tsis muaj kev tshaj tawm -weld heat treatment (PWHT). Rau cov refineries, qhov loj -scale daws annealing ntawm welded assemblies yog feem ntau impractical, cov cuab yeej no tsis yog tsuas yog qhov zoo xwb - nws yog ib tug tsim yuav tsum tau.

 

Qhov chaw: ASTM A276 / A276M-23 (Standard Specification for Stainless Steel Bars and Shapes); ATI 321/347/348 Technical Data Sheet; Carpenter Technology CarTech 321 Stainless Hlau Datasheet.

 

Element

Cov ntsiab lus (wt%)

Metallurgical Function

Cov pa roj carbon (C)

<= 0.08

Tswj tsis tshua muaj carbon rau weldability

Chromium (Cr)

17.0 - 19.0

Corrosion tsis kam; passive oxide txheej

Nickel (Ni)

9.0 - 12.0

Stabilizes austenitic qauv

Titanium (Ti)

5x(C+N) min, 0.70 max

Tiv thaiv chromium carbide nag lossis daus

Manganese (Mn)

<= 2.00

Deoxidizer; txhim kho kev ua haujlwm kub

Silicon (Si)

<= 1.00

Txhim kho oxidation tsis kam

Phosphorus (P)

<= 0.045

impurity txwv

Sulfur (S)

<= 0.030

impurity txwv

Hlau (Fe)

Tshuav

Base matrix

 

Vim li cas Creep Teebmeem hauv Kev Pabcuam Refinery?

 

Creep yog qhov tseem ceeb tsis ua hauj lwm mechanism rau siab- khaws cov khoom ua kom zoo tshaj 538 degrees C (1000 degrees F). Cov yeeb nkab lossis lub raj tuaj yeem tawg tsuas yog 40% ntawm nws chav- qhov kub thiab txias tawm lub zog tom qab 100,000 xuab moos ntawm kev pabcuam vim tias creep deformation accumulates dhau sijhawm - thiab ASME tus qauv tsim cov cai tswj kev nkag siab-raws li kev tso cai rau cov kev kub ntxhov no.

 

Why Does Creep Matter in Refinery Service

 

Txhais.Creep yog qhov qeeb, mus tas li deformation ntawm cov hlau nyob rau hauv kev ntxhov siab nyob rau hauv siab kub. Tsis zoo li kev ua tsis tiav tam sim ntawd, kev nkag mus ntsiag to nyob rau ntau xyoo. Cov txheej txheem tshwm sim nyob rau hauv peb theem:

 

Primary creep:cov khoom deforms sai sai tab sis ntawm tus nqi qis dua li cov tawv tawv tawv tiv thaiv ntxiv deformation.

 

Secondary (state{0}}state) nkag:tus deformation tus nqi yuav kwv yees li qhov tsis tu ncua - qhov no yog lub sijhawm ntev tshaj plaws thiab lub hauv paus rau feem ntau cov ntaub ntawv tsim qauv engineering.

 

Tertiary creep:deformation nrawm nrawm, ua rau caj dab thiab tawg. Kev tsim qauv yuav tsum khaws cov khoom tawm ntawm theem no.

 

Yog vim li cas Yield Strength Ib leeg tsis txaus.Refinery rhaub cov raj, cov kav dej hloov kho, thiab cov khoom siv hluav taws xob hloov pauv ib txwm ua haujlwm ntawm 538-870 ° C nyob rau hauv siab. Ntawm cov kub no, cov hlau tawm los lub zog tsis yog qhov txwv tsis pub dhau - creep zog yog. Ib lub raj uas dhau qhov kev ntsuas hydrostatic ntawm qhov kub thiab txias tuaj yeem ua tsis tiav tom qab 10-15 xyoo ntawm kev pabcuam kub kub yog tias tsis tau suav rau hauv kev tsim.

 

High School-Level Analogy.Ib qho piv txwv rau tsis yog{0}} cov kws tshaj lij: xav txog kev khoov tus kav yas thiab tuav nws hauv txoj haujlwm. Nws tsis snap, tab sis dhau sij hawm nws maj mam siv sij hawm mus tas li thiab tsis rov qab mus ncaj. Nyob rau hauv qhov kub thiab txias, steel coj zoo ib yam li nyob rau hauv kev ruaj ntseg load - nws maj mam stretches, thins, thiab nws thiaj li ruptures.

 

Source: ASME Boiler thiab Pressure Vessel Code, Tshooj VIII Division 1 (2023 Edition); ScienceDirect - Resistant Alloy (cov ntaub ntawv refinery siv).

 

Dab tsi yog Qhov Tseem Ceeb Creep Properties ntawm 321 Stainless Hlau?

 

321 stainless hlau tuav lub 100,000-teev creep rupture zog ntawm kwv yees li 90 MPa ntawm 600 degrees C thiab 50 MPa ntawm 650 degrees C. Rau 1% creep nyob rau hauv 100,000 teev, qhov tso cai rau kev ntxhov siab poob rau kwv yees li 80 MPa ntawm 650 degrees C thiab txhawb nqa tus nqi - 20-xyoo tsim lub neej rau refinery siab Cheebtsam nyob rau hauv 538-816 degrees C.

 

Cov lus hauv qab no suav nrog cov ntaub ntawv nkag los ntawm ntau qhov chaw tso cai, suav nrog ASME Tshooj II-D (2023), ATI Technical Data Sheets, Carpenter Technology datasheets, thiab luam tawm kev lag luam creep curves. Tus nqi sawv cev rau cov khoom siv kho mob annealed.

 

Table 1. Qhov Nruab Nrab Nruab Nrab Sib Nqus Rupture Stress rau 321 Stainless Hlau (MPa)

 

Kub

1,000 h Rupture

10,000 h Rupture

100,000 h Rupture

500 ° C (932 ° F)

~ 270 MPa

~ 240 MPa

~ 200 MPa

550 ° C (1022 ° F)

~ 220 MPa

~ 180 MPa

~ 120 MPa

600 ° C (1112 ° F)

~ 180 MPa

~ 130 MPa

~ 90 MPa

650 ° C (1202 ° F)

~ 140 MPa

~ 90 MPa

~ 50 MPa

700 ° C (1292 ° F)

~ 70 MPa

~ 50 MPa

~ 15 MPa

750 ° C (1382 ° F)

~ 45 MPa

~ 28 MPa

~ 5 MPa

800 ° C (1472 ° F)

~ 30 MPa

~ 10 MPa

~ 5 MPa

 

Table 2. Kev ntxhov siab los tsim 1% Creep hauv 321 Stainless Hlau (MPa)

 

Kub

1% Creep / 1,000 h

1% Creep / 10,000 h

1% Creep / 100,000 h

538 ° C (1000 ° F)

~ 155 MPa

~ 117 MPa

~ 75 MPa

550 ° C (1022 ° F)

~ 140 MPa

~ 100 MPa

~ 65 MPa

593 ° C (1100 ° F)

~ 100 MPa

~ 75 MPa

~ 48 MPa

600 ° C (1112 ° F)

~ 90 MPa

~ 60 MPa

~ 38 MPa

649 ° C (1200 ° F)

~ 60 MPa

~ 40 MPa

~ 19 MPa

650 ° C (1202 ° F)

~ 58MPa

~ 38 MPa

~ 18 MPa

704 ° C (1300 ° F)

~ 35 MPa

~ 22 MPa

~ 9 MPa

760 ° C (1400 ° F)

~ 18 MPa

~ 10 MPa

~ 4 MPa

Kev Pom Zoo.Cov ntaub ntawv qhia tau hais tias qhov sib txawv: rau txhua 50 ° C nce siab tshaj 550 ° C, creep rupture zog poob los ntawm kwv yees li 40-50%. Ntawm 700 ° C, 100,000-teev kev ntxhov siab rupture poob rau 15 MPa - lub ntsiab lus lub raj tsim rau 20-xyoo lub neej ntawm qhov kub no yuav xav tau cov phab ntsa tuab dua lossis qib siab dua alloy.

 

Cov peev txheej: ASME Boiler thiab Pressure Vessel Code Tshooj II-D (2023); ATI 321/347/348 Technical Data Sheet; Carpenter Technology CarTech 321 Datasheet; Corten Steels Alloy 321 Cov ntaub ntawv. Cov txiaj ntsig yog qhov zoo rau kev daws teeb meem- cov khoom siv annealed thiab yuav tsum tau txheeb xyuas nrog cov ntawv pov thawj zeb xeem ntawv (MTR) rau cov cai- qauv tsim.

 

Ua li cas 321 Stainless Steel piv rau 304, 316, thiab 347 ntawm Kub Kub?

 

321 stainless hlau muaj 15-25% siab dua creep rupture zog tshaj 304 thiab yog piv rau 347 hauv qab 650 degrees C. Rau refinery cov kev pab cuam yuav tsum welded sib dhos nyob rau hauv lub 425-870 degrees C ntau yam, 321 yog qhov zoo tshaj plaws tshuav nyiaj li cas ntawm creep zog, corrosion kuj, weldability tshaj 13, thiab tus nqi siab tshaj 10. rau kev pabcuam thermal cycling.

 

Table 3. Comparative Creep Rupture Strength ntawm 100,000 Teev (MPa)

Kub

304/304L

321

316/316L

347

500 ° C

~ 170 MPa

~ 200 MPa

~ 175 MPa

~ 210 MPa

550 ° C

~ 100 MPa

~ 120 MPa

~ 105 MPa

~ 130 MPa

600 ° C

~ 70 MPa

~ 90 MPa

~ 75 MPa

~ 95 MPa

650 ° C

~ 35 MPa

~ 50 MPa

~ 40 MPa

~ 55 MPa

700 ° C

~ 12 MPa

~ 15 MPa

~ 15 MPa

~ 18 MPa

 

321 vs 304/304L.304 thiab 304L yog cov qib austenitic hauv paus. Lawv tsis muaj stabilization, yog li ntev raug nyob rau hauv 425-815 degrees C ntau yam ua rau chromium carbide nag lossis daus thiab intergranular corrosion. 304L's low carbon (<=0.03%) slows sensitization but also reduces creep strength - ASME limits 304L to 425 degrees C (800 degrees F) for code applications. 321, with titanium stabilization, is rated to 816 degrees C (1500 degrees F).

 

321 vs 316/316L.316 ntxiv 2-3% molybdenum, uas txhim kho kev tiv thaiv pitting thiab crevice corrosion nyob rau hauv ib puag ncig chloride. Txawm li cas los xij, molybdenum tsis ua kom muaj zog nkag siab zoo piv rau titanium stabilization. Rau cov kev pab cuam refinery dominated los ntawm thermal cycling es tsis chloride raug, 321 yog nyiam. Qhov twg chloride corrosion yog thawj qhov kev txhawj xeeb (xws li, seawater-cooled exchangers), 316 yog qhov kev xaiv zoo dua.

 

321v 347 ib.347 siv niobium (columbium) hloov titanium rau stabilization. Ntawm qhov kub siab tshaj 650 ° C, 347 muab 10-20% siab dua creep rupture zog dua 321, thiab niobium carbides ruaj khov dua ntawm qhov kub siab heev. Txawm li cas los xij, 321 muaj cov qauv zoo dua rau qhov sib sib zog nqus kos thiab feem ntau yog 10-20% tsawg dua. Rau refinery cua sov raj hauv qab 650 ° C, 321 yog qhov kev xaiv zoo; rau cov raj superheater siab tshaj 650 degrees C, 347 lossis 321H yuav raug teev tseg.

 

Cov peev txheej: ASME Tshooj II-D (2023) tso cai rau cov lus ntxhov siab; ATI 321/347/348 Technical Data Sheet; Nickel Lub Tsev Kawm Ntawv Tshaj Tawm 9004 (High-Tsuas Yam Ntawm Cov Hlau Stainless).

 

Qhov Kev Pab Cuam Tshaj Plaws Tshaj Li Cas 321 tuaj yeem muaj txiaj ntsig hauv Kev Pabcuam Refinery?

 

What Maximum Service Temperatures Can 321 Sustain in Refinery Service

 

321 stainless hlau yog ntsuas rau kev pabcuam txuas mus txog 816 degrees C (1500 degrees F) thiab kev pabcuam cuam tshuam txog li 900 degrees C (1650 degrees F) nyob rau hauv oxidizing tej yam kev mob, nrog rau kev nyab xeeb ntsuas kub ntawm 871 degrees C (1600 degrees F). Rau ASME code daim ntawv thov, qhov siab tshaj plaws siv kub yog 816 degrees C (1500 degrees F).

Qhov xwm txheej

Max kub

Sau ntawv

Kev pabcuam txuas ntxiv (oxidizing)

816 ° C / 1500 ° F

ASME code siab tshaj plaws; scaling -zoo

Kev pabcuam cuam tshuam

900 ° C / 1650 ° F

Thermal cycling; luv dua

Safe scaling kub

871 ° C / 1600 ° F

saum toj no, oxide nplai loj hlob sai

ASME code max (Tshooj VIII)

816 ° C / 1500 ° F

Siab lub nkoj tsim txwv

Sensitization -ntau yam dawb

425-870 ° C / 800-1600 ° F

Ti stabilization tiv thaiv Cr-carbide

 

Environmental Considerations.Cov kev txwv kub no xav tias oxidizing ib puag ncig. Hauv kev pab cuam refinery, sulfur-cov roj muaj roj nyob rau hauv kev txo qis tuaj yeem ua kom nrawm nrawm ntawm austenitic stainless hlau. Nyob rau hauv ib puag ncig uas muaj H2S lossis SO2 ntawm qhov kub siab tshaj 650 ° C, kev sim ntsuas tau pom zoo ua ntej yuav tsum tau qhia 321, thiab siab dua -nickel alloys yuav tsum tau.

 

Qhov chaw: AZoM - Stainless Steel High Temperature Resistance (ASM Metals Handbook reference); Ntoor Technology CarTech 321 Datasheet; ATI 321/347/348 Technical Data Sheet.

 

Thaum twg Koj Yuav Tsum Hloov Kho ntawm 321 rau 321H rau Creep Service?

 

Hloov kho mus rau 321H (UNS S32109) thaum ua haujlwm kub siab tshaj 538 degrees C (1000 degrees F) nyob rau hauv kev ua haujlwm ruaj khov. 321H muaj cov ntsiab lus carbon ntau dua (0.04-0.10%) thiab cov nplej ntxhib loj (ASTM 7 lossis coarser), uas ua ke muab 10-20% kev thuam ntau dua 321 - 20-xyoo tsim lub neej nyob rau hauv refinery siab cov cuab yeej.

Khoom

321 (NWS S32100)

321 H (UNS S32109)

Cov ntsiab lus carbon

<= 0.08%

0.04 - 0.10%

Grain loj yuav tsum tau

Tsis tau teev tseg

ASTM 7 los yog coarser

ASME Tshooj I (boilers)

Tsis tsim nyog

Tsim nyog

ASME Section VIII Div. 1

Tsim nyog

Tsim nyog

ASME Section VIII Div. 2

Tsis tsim nyog

Tsim nyog

Max code kub

816 ° C (1500 ° F)

816 ° C (1500 ° F)

Yam hwm

Lub hauv paus

+10-20% tshaj 321

 

Metallurgical Rationale.Cov pa roj carbon ntau dua hauv 321H nce lub zog nkag los ntawm carbide nag lossis daus ntxiv zog - cov pa roj carbon monoxide yaj cov ntaub ntawv zoo carbides uas pin lis ciam teb thiab tiv thaiv cov nplej zawv zawg, ib qho tseem ceeb creep mechanism. Cov nplej ntxhib loj (ASTM grain loj 7 lossis loj dua, txhais tau tias tsawg dua, cov nplej loj dua) ntxiv rau kev nkag siab ntxiv vim tias cov qoob loo ciam teb zawv zawg yog qhov tseem ceeb ntawm cov txheej txheem nkag ntawm qhov kub thiab txias.

 

Kev pom zoo ntawm kev yuav khoom.Order 321/321H dual{2}}cov ntaub ntawv pov thawj thaum tsis paub meej txog cov kev pabcuam yav tom ntej. Ob daim ntawv pov thawj txhais tau tias cov cua sov ua tau raws li 321 (C<= 0.08%) and 321H (C = 0.04-0.10%, grain size ASTM 7+) specifications. The MTR must explicitly state the grain size and solution-annealing temperature (>=1038 degrees C) kom tsim nyog rau 321H ASME tso cai.

 

API 530 Kev txiav txim siab.API 530 (Xaiv lub rhaub Tube Thickness nyob rau hauv Refineries) yuav tsum tau creep-rupture-raws li tsim rau cov cua sov raj. Yog tias koj lub raj tsim kub siab tshaj 538 ° C thiab cov khoom siv thauj khoom (siab lossis hnyav), 321H yog qhov yuav tsum tau ua. Yog tias qib 321- qib tivthaiv tsuas yog xav tau kev tiv thaiv kev kub ntxhov siab tsis muaj qhov tseem ceeb (piv txwv li, lub tshuab hluav taws xob hauv ob sab phlu), tus qauv 321 txaus.

 

Source: ASME Boiler thiab Pressure Vessel Code Tshooj II-D (2023); API 530 (Xaiv ntawm Rhaub Tube Thickness hauv Petroleum Refineries); Kev lag luam kev lag luam cov txheej txheem rau 321/321H dual ntawv pov thawj.

 

Cov Cheebtsam Refinery feem ntau siv 321 Stainless Hlau?

 

321 stainless hlau yog dav siv nyob rau hauv refinery rhaub tubing, tshav kub exchanger tubing, FCC unit internals, catalytic hydrodesulfurization unit piping, amine unit Cheebtsam, sulfur rov qab unit piping, transformer tubes, thiab expansion pob qij txha - yeej tseem zoo ib yam kev tivthaiv kev khiav hauj lwm nyob rau hauv lub 425-870 degrees welded ib tug ntau yam.

Chav tsev Refinery

Tej Cheebtsam

Kev pab Temp Range

Yog vim li cas 321?

Lub tshuab cua sov

Tube txhawb, radiant seem raj

500-870 ° C

Creep zog + Ti stabilization

FCC chav tsev

Cyclone diplegs, swb li qub, standpipes

550-750 ° C

Thermal cycling tsis kam

Reformer

Piping, catalyst tubes, manifolds

500-700 ° C

Creep + intergranular corrosion

HDS unit

Reactor internals, tshav kub exchanger bundles

350-450 ° C

H2S tsis kam + weldability

Amine tsev

Rich / lean amine piping, exchangers

100-150 ° C

Welded yam tsis muaj PWHT

Sulfur rov qab

Claus tshuaj tiv thaiv rauv tub

300-650 ° C

Sulfidation + thermal stability

Hydrogen cog

Hloov kab, manifold piping

400-800 ° C

Creep + oxidation tsis kam

Distillation

Sab hauv sab hauv, lub tais txhawb nqa kab teeb

200-400 ° C

Intergranular corrosion kuj

 

Sour Service Qualification.321 kuj tseem yog NACE MR0175 / ISO 15156 pom zoo rau kev pabcuam qaub, ua rau nws tsim nyog rau cov chaw ua haujlwm refinery qhov twg H2S nyob. Qhov kev tsim nyog ob npaug no - rau ob qho tib si siab -kub creep thiab qaub qhov kev pabcuam - yog qhov laj thawj tseem ceeb 321 yog qib ua haujlwm hauv kev ua haujlwm qis.

 

Qhov chaw: ScienceDirect - Resistant Alloy (refinery austenitic stainless hlau daim ntawv thov); NACE MR0175 / ISO 15156 (kev pabcuam qaub ncaug); Tesco Steel 321/321H Flanges Cov Ntaub Ntawv

 

Yuav ua li cas ASME Code tso cai rau kev ntxhov siab rau 321 Kev Txhawb Kev Tsim Kho Kev Tsim Kho?

 

ASME Tshooj II-D (2023 tsab) muab 321 stainless hlau tso cai rau kev ntxhov siab ntawm 117 MPa ntawm 500 degrees C, 105 MPa ntawm 550 degrees C, 52 MPa ntawm 600 degrees C, 32 MPa ntawm 650 degrees C, thiab 18 MPa ntawm 18 MPa siab ntawm 70 degrees C. Cov txiaj ntsig no tau muab ncaj qha los ntawm cov ntaub ntawv nkag mus rau qhov tawg thiab txhais cov kev ntxhov siab siab tshaj plaws tau tso cai rau hauv cov cai- cov khoom siv ua raws li cov khoom siv refinery.

 

How Do ASME Code Allowable Stresses for 321 Support Refinery Design

 

Table 4. ASME Seem II-D (2023) Tso cai Stresses rau 321 Stainless Hlau

 

Kub

Tso cai Stress (MPa)

Hauv paus

100,000h Repture (xws li.)

500 ° C (932 ° F)

117 MPa

Tawm + tensile

~ 200 MPa

538 ° C (1000 ° F)

~ 95 MPa

Hloov mus rau creep

~ 160 MPa

550 ° C (1022 ° F)

105 MPa

Creep{0}} tswj tau

~ 120 MPa

600 ° C (1112 ° F)

52 MPa ua

Creep{0}} tswj tau

~ 90 MPa

649 ° C (1200 ° F)

~ 35 MPa

Creep{0}} tswj tau

~ 50 MPa

650 ° C (1202 ° F)

32 MPa

Creep{0}} tswj tau

~ 50 MPa

700 ° C (1292 ° F)

18 MPa

Creep{0}} tswj tau

~ 15 MPa

750 ° C (1382 ° F)

10 MPa

Creep{0}} tswj tau

~ 5 MPa

 

Yuav Ua Li Cas Tso Cai Kev Nyuaj Siab Tau Txais.Hauv qab kwv yees li 538 ° C, qhov kev ntxhov siab tso cai yog tswj hwm los ntawm qhov qis ntawm cov txiaj ntsig tau muab faib los ntawm kev nyab xeeb los yog lub zog tensile faib los ntawm kev nyab xeeb. Tshaj 538 degrees C, creep dhau los ua cov txheej txheem tswj hwm, thiab kev ntxhov siab tso cai tau los ntawm cov ntaub ntawv creep rupture - feem ntau 100,000-teev rupture lub zog muab faib los ntawm ib qho kev nyab xeeb ntawm kwv yees li 1.5 txog 3.0, nyob ntawm cov cai seem. Qhov kev hloov pauv no yog vim li cas 321H (nrog nws lub zog nkag siab dua) ua qhov tseem ceeb tshaj 538 degrees C.

 

Tsim Daim Ntawv Thov.Rau ASME B31.3 txheej txheem piping, zoo sib xws kev ntxhov siab siv tau. Tus tsim qauv siv cov txiaj ntsig no hauv cov qauv phab ntsa tuab: t=P x D / (2S + 2P), qhov twg P yog tsim siab, D yog sab nraud txoj kab uas hla, thiab S yog qhov tso cai rau kev ntxhov siab ntawm qhov tsim kub. Raws li kub nce thiab S poob, phab ntsa thickness yuav tsum nce proportionally - los yog siab dua -qib alloy yuav tsum tau xaiv.

 

Source: ASME Boiler thiab Pressure Vessel Code Tshooj II-D (2023 tsab), Table 1A (austenitic stainless hlau); ASME B31.3 Txheej Txheem Piping Code.

 

Dab tsi yog Cov Kev Cai Zoo Tshaj Plaws rau Vuam thiab Fabricating 321 hauv Kev Pabcuam Refinery?

 

321 stainless hlau tuaj yeem welded los ntawm txhua txoj hauv kev (TIG, MIG, submerged arc) siv ER347 muab tub lim hlau yam tsis muaj ncej-weld kev kho cua sov, vim tias titanium stabilization tiv thaiv rhiab heev hauv tshav kub- thaj tsam cuam tshuam. Siv ER347 (tsis yog ER308 los yog ER321) muab tub lim hlau los xyuas kom meej qhov vuam tso nyiaj kuj ruaj khov tiv thaiv carbide nag lossis daus.

 

Filler hlau xaiv:ER347 (niobium{1}}stabilized) yog tus qauv muab tub lim rau 321 puag hlau. Titanium nyob rau hauv ER321 muab tub lim yog nquag oxidation thaum lub sij hawm vuam, ua rau inconsistent stabilization. ER347 muab kev txhim khu kev qha, oxidation-tiv taus stabilization nyob rau hauv cov vuam deposit.

 

Tsis xav tau PWHT:321 yuav tsum tsis muaj ncej-weld tov annealing rau intergranular corrosion kuj. Qhov no yog qhov zoo tshaj plaws tshaj 304, uas yuav tsum tau PWHT tom qab vuam nyob rau hauv hnyav seem kom rov qab corrosion kuj.

 

Kub input tswj:Khaws qhov kub ntawm qhov kub ntawm 150 ° C thiab siv cov hlaws dai ntau dua li cov hlaws dav dav kom txo qis cov cua sov. Cov cua kub ntau dhau ua rau thaj chaw rhiab heev hauv HAZ.

 

Txheej txheem kev tsim nyog:Tsim nyog cov txheej txheem vuam rau ASME Tshooj IX. Rau siab - qhov kev pab cuam kub siab tshaj 538 degrees C, creep- kev ntsuam xyuas tawg ntawm vuam tej zaum yuav tsum tau ua ib qho kev hloov pauv tseem ceeb ntxiv.

 

Ncej -welding tu:Tom qab vuam, tshem tawm tag nrho cov slag, oxides, thiab cua sov tint los ntawm kev sib tsoo los yog pickling. Thaum tshav kub kub tint ntawm austenitic stainless hlau txo corrosion kuj nyob rau hauv cov cheeb tsam cuam tshuam.

 

Ua haujlwm txias thiab tawv.321 tsis tuaj yeem hardened los ntawm kev kho cua sov - tsuas yog los ntawm kev ua haujlwm txias. Rau cov khoom siv hluav taws xob uas xav tau lub zog siab dua, txias- cov kab kos lossis cov phaj tuaj yeem raug teev tseg, tab sis tus tsim qauv yuav tsum suav rau qhov txo qis thiab xyuas kom meej tias kev ua haujlwm txias tsis cuam tshuam rau kev ua haujlwm ntawm qhov kub thiab txias (kev ntxhov siab yuav tshwm sim).

 

Cov peev txheej: ATI 321/347/348 Technical Data Sheet (welding recommendations); AWS A5.9 (Bare welding electrodes); Tesco Steel 321/321H Flanges kev qhia; ASME Section IX (welding txheej txheem tsim nyog).

 

Ntev npaum li cas -Lub Sij Hawm Thermal Aging cuam tshuam rau 321 Stainless Hlau?

 

321 stainless hlau resists sigma-theem embrittlement zoo dua li siab dua -chromium qib zoo li 310 lossis 316, tab sis ntev raug tshaj 650 degrees C rau ntau tshaj 50,000 teev yuav tsum tau saib xyuas kev puas tsuaj, microstructural degradation, thiab muaj peev xwm sigmase{8} Kev kuaj tsis tu ncua tsis tu ncua yog qhov tseem ceeb rau cov khoom mus txog qhov kawg ntawm lub neej tsim.

Hnub nyoog Risk

Qhov kub thiab txias

Qhov pib

Kev txo qis

Sigma theem tsim

590-870 ° C

>50,000 h raug

321 tsawg dua 310/316; saib xyuas

Carbide coarsening

>600 ° C

Ntev -lub sij hawm

TiC ruaj khov dua Cr-carbide

Creep cavitation

>538 ° C nyob rau hauv kev ntxhov siab

>100,000 h

NDE: ultrasonic, replication

Sensitization (rov qab)

425-815 ° C

Nquag tiv thaiv los ntawm Ti

Txheeb xyuas Ti/C piv rau MTR

Cov qoob loo loj hlob

>900 ° C

Kev nphav raug los ntev lawm

Tswj los ntawm zeb annealing

 

Sigma-Phase Embrittlement.Sigma phase is a hard, brittle intermetallic compound (FeCr) that can form in austenitic stainless steels during long exposure to temperatures between 590 and 870 degrees C. Grade 304 is nearly immune due to its lower chromium content. Grade 321 is less susceptible than 310 or 316 because titanium restricts chromium mobility, but very long exposures (>50,000 hours at >650 ° C) tseem tuaj yeem ua rau nag lossis daus. Yog tias pom tau tias sigma{2}}theem embrittlement, nws tuaj yeem yaj tau los ntawm re-annealing ntawm 1038 degrees C yam tsawg kawg nkaus - tab sis qhov no tsis tshua muaj txiaj ntsig rau hauv - cov khoom siv ua haujlwm refinery.

 

Kev soj ntsuam cov lus pom zoo.Rau refinery Cheebtsam mus txog lawv lub neej tsim, pom zoo NDE suav nrog: ultrasonic thickness ntsuas (los taug qab creep thinning), deg replication (kom pom creep cavitation ntawm cov ciam teb), thiab hardness testing (los kuaj sigma-theem embrittlement, uas tsub kom hardness). API 530 thiab API 573 muab kev taw qhia txog kev ntsuas hluav taws xob hluav taws xob hluav taws xob thiab kev suav lub neej ntxiv.

 

Tau qhov twg los: AZoM - Stainless Steel High Temperature Resistance; API 530 (Rhaub Tube Thickness); API 573 (Tshuaj Rhaub Tshuaj Xyuas); NACE MR0103 (cov khoom siv ua kom zoo dua qub).

 

Cov lus nug nquag

 

Dab tsi yog qhov creep rupture zog ntawm 321 stainless hlau ntawm 600 degrees C?

Lub 100,000-teev creep rupture zog ntawm 321 stainless hlau ntawm 600 degrees C yog kwv yees li 90 MPa. Rau 10,000 teev, nws yog kwv yees li 130 MPa, thiab rau 1,000 teev, kwv yees li 180 MPa. Cov txiaj ntsig no suav tias yog kev daws teeb meem- cov khoom siv annealed thiab yuav tsum tau ua pov thawj tiv thaiv cov ntawv pov thawj zeb xeem ntawv rau kev tsim qauv raws cai.

 

321 stainless hlau puas tuaj yeem siv siab dua 800 degrees C?

321 stainless hlau tuaj yeem siv sib cuam tshuam txog 900 ° C (1650 ° F) rau oxidation tsis kam. Txawm li cas los xij, rau ASME code siab-cov ntawv thov, qhov siab tshaj plaws siv yog 816 degrees C (1500 degrees F). Tshaj 800 degrees C, creep rupture zog poob mus rau kwv yees li 5 MPa ntawm 100,000 teev, thiab siab dua-qib alloy xws li 310S los yog npib tsib xee{14}}raws li alloy (piv txwv li, Inconel 600) raug pom zoo rau kev thauj khoom tas mus li - kev pabcuam kabmob.

 

Dab tsi yog qhov txawv ntawm 321 thiab 321H stainless hlau?

321H (UNS S32109) muaj cov ntsiab lus carbon ntau dua (0.04-0.10% vs<=0.08% for standard 321) and requires a coarse grain size (ASTM 7 or coarser). These differences provide 10-20% higher creep rupture strength above 538 degrees C. 321H is qualified for ASME Section I (power boilers) and Section VIII Division 2, while standard 321 is limited to Section VIII Division 1. Order dual-certified 321/321H material when uncertain about future requirements.

 

Puas yog 321 stainless hlau haum rau kev pabcuam qaub hauv cov chaw ua haujlwm?

Tau. 321 stainless hlau yog NACE MR0175/ISO 15156 tau pom zoo rau kev pabcuam qaub, ua rau nws tsim nyog rau cov chaw ua haujlwm refinery qhov twg hydrogen sulfide (H2S) nyob. Nws kev sib xyaw ua ke ntawm siab - qhov kub thiab txias creep zog, intergranular corrosion kuj, thiab qaub kev pab cuam tsim nyog yog ib tug tseem ceeb vim li cas nws yog dav teev nyob rau hauv downstream refining, tshwj xeeb tshaj yog nyob rau hauv hydrodesulfurization units, amine units, thiab sulfur rov qab units.

 

Kuv puas yuav tsum xaiv 321 lossis 347 rau siab -kub refinery kev pabcuam?

Xaiv 321 rau cov kev pab cuam refinery hauv qab 650 degrees C uas tus nqi -effectiveness thiab formability yog qhov tseem ceeb. Xaiv 347 rau kev pabcuam siab tshaj 650 ° C qhov siab tshaj plaws creep lub zog yog qhov tseem ceeb, lossis nyob rau hauv ib puag ncig nuclear uas yuav tsum zam kev ua kom titanium. Ob qib yog titanium/niobium-stabilized thiab tiv thaiv intergranular corrosion nyob rau hauv 425-870 degrees C ntau, tab sis 347 muab 10-20% siab dua creep rupture zog ntawm tus nqi ntawm 10-20% tus nqi siab dua.

 

Xaus

 

321 stainless hlau tseem yog cov khoom siv pob zeb rau kev ua kom zoo siab - kev pabcuam kub. Nrog 100,000-teev creep rupture muaj zog ntawm 90 MPa ntawm 600 degrees C thiab 50 MPa ntawm 650 degrees C, ASME code tsim nyog rau 816 degrees C, thiab NACE qaub kev pab cuam pom zoo, nws muab cov kev sib txuas ntawm creep kuj, weldability, thiab corrosion tiv thaiv uas refinery siab cov khoom xav tau.

 

Rau engineers thiab procurement managers qhia cov ntaub ntawv rau refinery kev pab cuam nyob rau hauv lub 425-870 degrees C ntau yam, 321 stainless hlau muaj ib tug proven, code{3}}raws li, thiab nqi-zoo tshuaj. Cov ntsiab lus tseem ceeb ntawm kev txiav txim siab ncaj nraim: siv tus qauv 321 hauv qab 538 degrees C; hloov mus rau 321H saum toj no 538 degrees C nyob rau hauv kev ruaj ntseg load; xav txog 347 saum toj no 650 ° C rau siab tshaj plaws creep zog; thiab nce mus txog 310S lossis npib tsib xee alloys saum 900 degrees C.

 

Xav tau ntawv pov thawj 321 lossis 321H stainless hlau rau koj qhov project refinery?Hu rau peb pab pawg kws tshaj lij rau cov khoom siv tshwj xeeb, cov ntawv xeem ntsuas, thiab ASME code-raws li cov khoom siv ntawm 321/321H stainless hlau tuav, phaj, kav dej, thiab flanges - txhawb nqa los ntawm tag nrho traceability thiab NACE MR0175 ntawv pov thawj.

 

Xa kev nug
Los rau peb
Thiab pib koj rfqs tam sim no.
Tiv Tauj Peb